Modified diaphragm with flame-retardant capability and strong mechanical property and preparation method of modified diaphragm
By using the interaction of polymers, phosphate ester flame retardants and solid electrolytes in secondary battery separators to construct coatings, the problems of easy melting and high cost of flame retardants in the existing technology are solved, and excellent separators are achieved. Flame retardant and mechanical properties improve battery safety and cycle stability.
Patent Information
- Application Number
- CN202410895413.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-07-04
AI Technical Summary
The flame retardant in the existing secondary battery separator is easy to melt at high temperatures and cannot effectively prevent thermal runaway. At the same time, the cost is high, and it is difficult to prevent the flame retardant from reducing at the negative electrode without affecting the battery function.
A coating including polymer, phosphate flame retardant, solid electrolyte, wetting agent and binder is used. Through the interaction between solid electrolyte and phosphate flame retardant, the flame retardant is fixed and the crystallinity of the polymer is reduced. , enhance the mechanical properties and adhesion of the separator, and avoid the reduction of flame retardants at the negative electrode.
It is possible to improve the flame retardancy and mechanical properties of the separator without affecting the battery function, prevent thermal runaway, reduce the internal resistance of the battery, and improve the safety and cycle stability of the battery core.
Smart Images

Figure BDA0004930127950000111 
Figure HDA0004930128140000011
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of secondary batteries, and in particular relates to a modified diaphragm with flame retardancy and strong mechanical properties and a preparation method thereof. Background Art
[0002] A secondary battery, also known as a rechargeable battery or storage battery, is a battery that can be recharged to activate the active material and continue to be used after the battery is discharged. The rechargeable characteristics of secondary batteries and their efficient and stable energy conversion capabilities make them one of the key technologies in the field of modern power applications. They are widely used in electric vehicles, electric bicycles, energy storage systems and other occasions that require high power output or long-term continuous power supply.
[0003] The extremely high energy density and integration density of power batteries mean that once thermal runaway occurs, the battery will catch fire quickly or even explode. When the temperature inside the battery rises abnormally, the electrolyte decomposes to produce a large number of hydrogen radicals, which react with the oxygen released by the positive electrode active material to release a large amount of heat and trigger a chain reaction, leading to thermal runaway of the battery. Adding flame retardants to consume hydrogen radicals to block chain reactions and thermal runaway has been widely verified to be a feasible solution, but commonly used cheap flame retardants such as TEP and TMP have poor reduction resistance and are easily reduced at the negative electrode, causing SEI thickening, which in turn affects the battery capacity.
[0004] A Chinese patent with publication number CN115939661A discloses a process for preparing a sodium ion battery coated diaphragm, in which poly(vinylidene fluoride-co-hexafluoropropylene) (PVDF-HFP) is doped and mixed with polyethylene oxide (PEO) and boehmite, wherein the boehmite provides a skeleton support to ensure the mechanical strength of the diaphragm, and at the same time forms a three-dimensional porous grid structure with PVDF-HFP and PEO, which greatly improves the ionic conductivity and can improve the first efficiency and rate performance; maleic anhydride is then added, and polar functional groups are introduced into the PVDF-HFP surface through a grafting reaction, and the adhesion between the PVDF-HFP and the negative electrode plate is improved through hydrogen bonding, and the peeling strength is improved, which can reduce the internal resistance of the battery and improve the cycle performance; finally, a coated diaphragm with high ionic conductivity and good adhesion to the positive and negative electrode plates is obtained through the above process. However, in order to improve the ionic conductivity of the diaphragm coating, this method uses PVDF-HFP, which has a high dielectric constant and is expensive, and compounds it with PEO, resulting in a high overall cost. In addition, in order to improve the adhesion of the diaphragm to the positive and negative electrodes, maleic anhydride is introduced, which has a low melting and boiling point. When the battery is running at high temperature, the melting of maleic anhydride may cause the polymer coating to peel off. It can be seen that the diaphragm provided by this patent cannot improve the safety performance of the battery. Although PVDF-HFP absorbs heat when it melts at high temperatures, its heat absorption capacity is limited and it cannot absorb heat in the early stage of the battery temperature rise to prevent thermal runaway.
[0005] There is currently no effective and low-cost way to integrate flame retardants such as TEP inside the battery to prevent reduction at the negative electrode without affecting its function. Summary of the invention
[0006] In view of this, the technical problem to be solved by the present invention is to provide a modified diaphragm with flame retardancy and strong mechanical properties and a preparation method thereof.
[0007] The present invention provides a modified diaphragm with flame retardancy and strong mechanical properties, comprising: a base film and a coating disposed on at least one surface of the base film;
[0008] The coating comprises a polymer, a phosphate flame retardant, a solid electrolyte, a wetting agent and a binder.
[0009] Preferably, the mass ratio of the polymer to the solid electrolyte is 1:(3-5).
[0010] Preferably, the coating is formed by slurry; the mass ratio of polymer to phosphate flame retardant in the slurry is 1:(11-15);
[0011] The mass of the wetting agent is 0.3% to 0.5% of the mass of the slurry;
[0012] The mass of the binder is 3% to 5% of the mass of the solid electrolyte.
[0013] Preferably, the polymer is selected from one or more of vinylidene fluoride-chlorotrifluoroethylene copolymer, polyvinyl fluoride, polyvinylidene fluoride, ethylene-chlorotrifluoroethylene copolymer, tetrafluoroethylene-hexafluoropropylene copolymer, ethylene-tetrafluoroethylene copolymer and tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer;
[0014] The phosphate flame retardant is selected from one or more of trimethyl phosphate, triethyl phosphate, tri(2,2,2-trifluoroethyl) phosphate, tri(1,3-dichloro-2-propyl) phosphate, diphenyl cresol phosphate and diphenyl monooctyl phosphate;
[0015] The solid electrolyte is selected from a lithium solid electrolyte or a sodium solid electrolyte;
[0016] The lithium solid electrolyte is selected from one or more of a lithium lanthanum zirconium oxide solid electrolyte, a lithium lanthanum titanium oxide solid electrolyte and a lithium aluminum titanium phosphate solid electrolyte;
[0017] The sodium solid electrolyte is selected from Na3AlF6, Na3ZrF6, Na2SiF6, Na 12 Al 12 Si 12 O 48, NZSP and Na-β / β”-Al2O3;
[0018] The wetting agent is one or more of an acetylenediol wetting agent and a polyether siloxane wetting agent;
[0019] The binder is selected from one or more of carboxymethyl acrylate, sodium carboxymethyl cellulose, polyacrylamide-based binders, polyvinyl alcohol-based binders, and PVDF-based binders.
[0020] Preferably, the coating has a thickness of 1 to 5 μm.
[0021] Preferably, the base film is selected from polypropylene film or polyethylene film; and the particle size of the solid electrolyte is 500-600 nm.
[0022] The present invention also provides a method for preparing the above-mentioned modified diaphragm having flame retardancy and strong mechanical properties, comprising the following steps:
[0023] Coating the slurry on at least one surface of the base membrane to obtain a modified diaphragm;
[0024] The slurry comprises a polymer, a phosphate flame retardant, a solid electrolyte, a wetting agent and a binder.
[0025] Preferably, the slurry is prepared according to the following method:
[0026] S1) mixing the solid electrolyte with a portion of the phosphate flame retardant to obtain slurry A;
[0027] The polymer is mixed with the remaining phosphate flame retardant to obtain slurry B;
[0028] S2) mixing the slurry A, slurry B, a wetting agent and a binder to obtain a slurry.
[0029] Preferably, the solid content of the slurry A is 50% to 60%; the mass ratio of the polymer to the remaining phosphate flame retardant in the slurry B is 1:(8-10).
[0030] The present invention also provides a secondary battery, comprising the modified diaphragm with flame retardancy and strong mechanical properties, a positive electrode and a negative electrode.
[0031] The present invention provides a modified diaphragm with flame retardant ability and strong mechanical properties, including: a base film and a coating disposed on at least one surface of the base film; the coating includes a polymer, a phosphate flame retardant, a solid electrolyte, a wetting agent and a binder. Compared with the prior art, the present invention constructs a diaphragm coating with good flame retardant ability and excellent mechanical properties through the interaction between the solid electrolyte, the polymer and the phosphate flame retardant. The interaction between the three allows a large amount of phosphate flame retardant solvent to remain in the coating, avoiding the reduction of phosphate flame retardant molecules at the negative electrode to generate a poor quality SEI layer, without affecting the release of phosphate flame retardant at high temperature to participate in flame retardancy; in addition, the interaction reduces the crystallinity of the polymer, and the coating with stronger viscosity is not easy to peel off in the battery system, and can improve the tightness of the combination with the positive and negative electrodes, prevent the diaphragm from wrinkling, and improve the consistency of the battery cell. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 This is a SEM image of the PVDF and solid electrolyte composite coated diaphragm obtained in Example 1 of the present invention. DETAILED DESCRIPTION
[0033] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] The present invention provides a modified diaphragm with flame retardancy and strong mechanical properties, comprising: a base film and a coating arranged on at least one surface of the base film; the coating comprises a polymer, a phosphate flame retardant, a solid electrolyte, a wetting agent and a binder.
[0035] The present invention fixes the phosphate flame retardant through the synergistic effect between the phosphate flame retardant and the solid electrolyte. For example, the phosphate flame retardant is TEP and the polymer is PVDF: TEP, as a cheap flame retardant, can block the free radical chain reaction inside the battery cell and avoid thermal runaway. However, if TEP is directly added to the electrolyte, it will be reduced at the negative electrode, resulting in a thicker SEI, which affects the cycle stability. The present invention first fixes the Li precipitated in the solid electrolyte + / Na +It forms a stable solvation structure with TEP molecules to fix the TEP solvent. Secondly, the high-valent metal ions in the solid electrolyte interact with TEP to produce an alkaline liquid environment. During the high-temperature drying process after the diaphragm is sprayed, PVDF is dehydrofluorinated and then cross-linked and gelled, reducing the crystallinity of PVDF to effectively accommodate the TMP solvent. In addition, PVDF contains a large amount of fluorine elements, is non-flammable, melts and absorbs heat at high temperatures, and the melted PVDF will block the pores of the diaphragm to avoid short circuits and thermal runaway. PVDF with poor crystallinity can fix solid electrolyte particles, enhance the tensile strength and puncture strength of the diaphragm, and thus effectively inhibit lithium dendrites.
[0036] According to the present invention, the modified diaphragm provided by the present invention includes a base film; the base film can be a base film well known to those skilled in the art without any special limitation, and in the present invention, it is preferably a polypropylene (PP) film or a polyethylene (PE) film.
[0037] According to the present invention, at least one surface of the base film is provided with a coating; the coating comprises a polymer, a phosphate flame retardant, a solid electrolyte, a wetting agent and a binder.
[0038] In a specific embodiment provided by the present invention, the polymer is a polymer well known to those skilled in the art without any special restrictions. In the present invention, it is preferably one or more of vinylidene fluoride-chlorotrifluoroethylene copolymer (VDF-CTFE), polyvinyl fluoride (PVF), polyvinylidene fluoride (PVDF), ethylene-chlorotrifluoroethylene copolymer (ECTFE), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), ethylene-tetrafluoroethylene copolymer (ETFE) and tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (PFA); the weight average molecular weight of the polymer is preferably 100,000 to 2 million, more preferably 500,000 to 1.5 million, and even more preferably 800,000 to 1 million.
[0039] In a specific embodiment provided by the present invention, the phosphate flame retardant is a liquid phosphate flame retardant well known to those skilled in the art, without any special restrictions. In the present invention, it is preferably one or more of trimethyl phosphate (TMP), triethyl phosphate (TEP), tri(2,2,2-trifluoroethyl) phosphate (TFP), tri(1,3-dichloro-2-propyl) phosphate (TDP), diphenyl cresol phosphate (CDP) and diphenyl octyl phosphate (DPOF).
[0040] In a specific embodiment provided by the present invention, the coating is formed by a slurry; the phosphate flame retardant in the slurry also serves as a solvent, and the mass ratio of the polymer to the phosphate flame retardant in the slurry is preferably 1: (11-15), more preferably 1: (12-15), and even more preferably 1: (13-15); in some embodiments provided by the present invention, the mass ratio of the polymer to the phosphate flame retardant in the slurry is specifically 1: 14, 1: 13 or 1: 15.
[0041] In a specific embodiment provided by the present invention, the solid electrolyte can be a solid electrolyte well known to those skilled in the art without any special restrictions. In the present invention, it is preferably a lithium solid electrolyte or a sodium solid electrolyte; the lithium solid electrolyte can be a lithium solid electrolyte well known to those skilled in the art without any special restrictions. In the present invention, it is preferably one or more of lithium lanthanum zirconium oxide solid electrolyte (LLZO), lithium lanthanum titanium oxide solid electrolyte (LLTO) and lithium aluminum titanium phosphate solid electrolyte (LATP); the sodium solid electrolyte is selected from Na3AlF6, Na3ZrF6, Na2SiF6, Na 12 Al 12 Si 12 O 48 , NZSP and Na-β / β"-Al2O3; the particle size of the solid electrolyte is preferably 500-600 nm; the mass ratio of the polymer to the solid electrolyte is preferably 1:(3-5); in some embodiments provided by the present invention, the mass ratio of the polymer to the solid electrolyte is specifically 1:3, 1:4 or 1:5.
[0042] In a specific embodiment provided by the present invention, the wetting agent can be a wetting agent well known to those skilled in the art without any special limitation. In the present invention, it is preferably one or more of acetylene glycol wetting agents and polyether siloxane wetting agents; the mass of the wetting agent is preferably 0.3wt% to 0.5wt% of the slurry mass.
[0043] In a specific embodiment provided by the present invention, the binder can be a binder well known to those skilled in the art without any special restrictions. In the present invention, it is preferably one or more of carboxymethyl acrylate, sodium carboxymethyl cellulose, polyacrylamide binders, polyvinyl alcohol binders and PVDF binders; the mass of the binder is preferably 3wt% to 5wt% of the mass of the solid electrolyte.
[0044] In a specific embodiment provided by the present invention, the thickness of the coating is preferably 1 to 5 μm, more preferably 1 to 4 μm, and even more preferably 2 to 3 μm.
[0045] In a specific embodiment provided by the present invention, coatings are provided on both surfaces of the base film; the thickness of the two coatings is preferably 1 to 5 μm, more preferably 1 to 4 μm, and even more preferably 2 to 3 μm, each independently.
[0046] The present invention constructs a diaphragm coating with good flame retardancy and excellent mechanical properties through the interaction between a solid electrolyte, a polymer and a phosphate flame retardant. The interaction between the three allows a large amount of phosphate flame retardant solvent to remain in the coating, thereby avoiding the reduction of phosphate flame retardant molecules at the negative electrode to generate a SEI layer of poor quality, without affecting the release of the phosphate flame retardant at high temperature to participate in flame retardancy; in addition, the interaction reduces the crystallinity of the polymer, and the coating with stronger viscosity is not easy to peel off in the battery system, and can improve the tightness of the combination with the positive and negative electrodes, prevent the diaphragm from wrinkling, and improve the consistency of the battery cell.
[0047] The present invention also provides a method for preparing the above-mentioned modified diaphragm with flame retardancy and strong mechanical properties, comprising the following steps: coating a slurry on at least one surface of a base film to obtain a modified diaphragm; the slurry comprises a polymer, a phosphate flame retardant, a solid electrolyte, a wetting agent and a binder.
[0048] Among them, the present invention has no special restrictions on the sources of all raw materials, as long as they are commercially available; the types and proportions of the polymer, phosphate flame retardant, solid electrolyte, wetting agent and binder are the same as described above and will not be repeated here.
[0049] In a specific embodiment provided by the present invention, the slurry is prepared according to the following method: S1) mixing a solid electrolyte with a part of a phosphate flame retardant to obtain slurry A; mixing a polymer with the remaining phosphate flame retardant to obtain slurry B; S2) mixing the slurry A, slurry B, a wetting agent and a binder to obtain a slurry.
[0050] In a specific embodiment provided by the present invention, the solid content of the slurry A obtained by mixing the solid electrolyte and part of the phosphate flame retardant is preferably 50% to 60%.
[0051] In a specific embodiment provided by the present invention, the mass ratio of the polymer to the remaining phosphate flame retardant is preferably 1:(5-15), and more preferably 1:(8-10).
[0052] In a specific embodiment provided by the present invention, the polymer and the remaining phosphate flame retardant are preferably mixed for 10 to 20 hours.
[0053] In a specific embodiment provided by the present invention, the slurry A and slurry B are mixed and then a wetting agent and a binder are added; the mass of the wetting agent is preferably 0.3wt% to 0.5wt% of the mass of the slurry; the mass of the binder is preferably 3wt% to 5wt% of the mass of the slurry.
[0054] The slurry is coated on at least one surface of the base film to obtain a modified diaphragm; the coating method is a method well known to those skilled in the art and is not particularly limited. In the present invention, spray coating is preferred.
[0055] The present invention also provides a secondary battery, comprising the modified diaphragm with flame retardancy and strong mechanical properties, a positive electrode and a negative electrode.
[0056] In a specific embodiment provided by the present invention, the active material of the positive electrode is preferably NCM811.
[0057] In a specific embodiment provided by the present invention, the active material of the negative electrode is preferably graphite.
[0058] In order to further illustrate the present invention, the modified diaphragm with flame retardancy and strong mechanical properties and the preparation method thereof are described in detail below in conjunction with embodiments.
[0059] The reagents used in the following examples are all commercially available; the PE base film used in the examples is a wet-pulled 9 μm isolation film with a porosity of 44%; the styrene-butadiene rubber is an SBR emulsion for lithium batteries (purchased from JSR Corporation of Japan); the polyacrylamide binder used in the examples is purchased from Tianjin Saipurui New Energy Technology Co., Ltd., the polyether-modified polysiloxane wetting agent is purchased from Guangdong Sandingjia New Materials Technology Co., Ltd., model SJD9006, and sodium carboxymethyl cellulose is purchased from Sichuan Lanyang Daily Chemical Co., Ltd.
[0060] Example 1
[0061] 1) Preparation of composite PVDF coated diaphragm:
[0062] The LLZO solid electrolyte is dispersed in TEP by a disperser to obtain slurry A, in which the LLZO particle size is 500-600nm and the solid content is 50%. PVDF (molecular weight of 1000000) is added to TEP to prepare slurry B, and the stirring time is 10h, in which the mass ratio of PVDF to TEP is 1:10. The prepared slurry A and slurry B are mixed in a ratio of PVDF:LLZO mass ratio of 1:4, and then a binder (polyacrylamide binder) of 5wt% of the LLZO mass and a wetting agent (polyether modified polysiloxane wetting agent) of 0.3wt% of the total mass of the slurry are added, and the prepared slurry is applied on the PE base film by spraying, and the coating thickness is controlled to be 2μm, and double-sided coating.
[0063] 2) Lithium-ion battery assembly:
[0064] NCM811 positive electrode active material (purchased from Ningbo Rongbai New Energy Technology Co., Ltd.), Super-p (purchased from Tianjin Huacai Chemical Co., Ltd.), and PVDF binder (HSV900 of Arkema) were added to NMP in a weight ratio of 96:1.5:2.5 and mixed evenly (solid content 72%). The positive electrode slurry was evenly coated on both surfaces of the aluminum foil (single-sided surface density of 15.8 mg / cm 2 ), further dried, rolled and cut to obtain the positive electrode sheet. The negative electrode active material graphite, Super-p, binder styrene-butadiene rubber, and thickener sodium carboxymethyl cellulose were added to the solvent deionized water (solid content 54%) according to a weight ratio of 96.2:0.8:0.8:1.2, and the mixed negative electrode slurry was evenly coated on both surfaces of the copper foil (single surface density 10mg / cm 2 ), and then the negative electrode sheet is obtained through drying, rolling and slitting.
[0065] The diaphragm is dried at 60°C for 48 hours, and the positive electrode, diaphragm, and negative electrode are stacked in order to obtain a battery cell assembly. After packaging, lithium ion electrolyte (LP30 electrolyte, with 5wt% fluoroethylene carbonate and 2wt% vinyl carbonate added) is injected. After packaging, standing, and forming, the battery cell is obtained. The rated capacity of the soft-pack battery cell is 1Ah, and the injection volume is 5g. The battery cell formation procedure is: charge at a current of 0.1C for 2 hours, then charge at a current of 0.2C to a cut-off voltage of 4.2V, and continue constant voltage charging until the current drops to 0.05C. Maintain 45°C and 10Kg / cm during formation. 2 heat pressing conditions.
[0066] To ensure data credibility, three cells were assembled in parallel and numbered as Examples 1.1 to 1.3.
[0067] Comparative Example 1
[0068] The preparation method of the lithium-ion battery cell in Comparative Example 1 is the same as that in Example 1, but the separator used is a PE-based film, and three batteries are assembled in parallel, which are numbered as Comparative Examples 1.1 to 1.3.
[0069] Comparative Example 2
[0070] The preparation method of the lithium-ion battery cell in Comparative Example 2 is the same as that in Example 1, but the diaphragm used is a PE diaphragm coated with a solid electrolyte only. The diaphragm coating scheme is as follows: the LLZO solid electrolyte is dispersed in TEP by a disperser, wherein the LLZO particle size is 500-600nm, and the solid content is 50wt%. After dispersion, 5wt% of the LLZO mass of the binder (polyacrylamide binder) and 0.3wt% of the total mass of the slurry (polyether modified polysiloxane wetting agent) are added, and it is applied on the PE base film by roller coating, and the coating thickness is controlled to be 2μm.
[0071] To ensure the credibility of the data, three cells were assembled in parallel and numbered as comparative examples 2.1 to 2.3.
[0072] Comparative Example 3
[0073] Only PVDF was used to coat the diaphragm, and the diaphragm coating scheme was as follows: PVDF was added to TEP to prepare a slurry, and the stirring time was 10 hours, wherein the mass ratio of PVDF to TEP was 1:10. 5wt% of sodium carboxymethyl cellulose and 0.3wt% of a wetting agent (polyether-modified polysiloxane wetting agent) were added to the prepared slurry, and the prepared slurry was applied to the PE base film by spraying, and the coating thickness was controlled to be 2μm, and double-sided coating was performed.
[0074] Example 2
[0075] The preparation method of lithium-ion battery is the same as that of Example 1, and the diaphragm coating scheme used is as follows: LLZO solid electrolyte is dispersed in TEP by a disperser to obtain slurry A, wherein the LLZO particle size is 500-600nm and the solid content is 50%. PVDF (molecular weight of 1000000) is added to TEP to form slurry B, and the stirring time is 10h, wherein the mass ratio of PVDF to TEP is 1:10. The configured slurry A and slurry B are mixed in a ratio of PVDF:LLZO mass ratio of 1:3, and then a binder (polyacrylamide binder) of 5wt% of the mass of LLZO and a wetting agent (polyether modified polysiloxane wetting agent) of 0.3wt% of the total mass of the slurry are added, and the configured slurry is applied on the PE base film by spraying, and the coating thickness is controlled to be 2μm, and double-sided coating is performed.
[0076] To ensure data credibility, three cells were assembled in parallel and numbered as Examples 2.1 to 2.3.
[0077] Example 3
[0078] The preparation method of lithium-ion battery is the same as that of Example 1, and the diaphragm coating scheme used is as follows: LLZO solid electrolyte is dispersed in TEP by a disperser to obtain slurry A, wherein the LLZO particle size is 500-600nm and the solid content is 50%. PVDF (molecular weight of 1000000) is added to TEP to form slurry B, and the stirring time is 10h, wherein the mass ratio of PVDF to TEP is 1:10. The configured slurry A and slurry B are mixed in a ratio of PVDF:LLZO mass ratio of 1:5, and then a binder (polyacrylamide binder) of 5wt% of the mass of LLZO and a wetting agent (polyether modified polysiloxane wetting agent) of 0.3wt% of the total mass of the slurry are added, and the configured slurry is applied on the PE base film by spraying, and the coating thickness is controlled to be 2μm, and double-sided coating.
[0079] To ensure data credibility, three cells were assembled in parallel and numbered as Examples 3.1 to 3.3.
[0080] Example 4
[0081] The preparation method of lithium-ion battery is the same as that of Example 1. The polymer used for coating the diaphragm is PTFE, and the flame retardant solvent is TMP. The scheme is as follows: LLZO solid electrolyte is dispersed in TMP by a disperser to obtain slurry A, wherein the LLZO particle size is 500-600nm and the solid content is 50%. PTFE (molecular weight of 1000000) is added to TMP to form slurry B, and the stirring time is 10h, wherein the mass ratio of PTFE to TMP is 1:10. The configured slurry A and slurry B are mixed in a ratio of PTFE:LLZO mass ratio of 1:4, and then a binder (polyacrylamide binder) of 5wt% of the mass of LLZO and a wetting agent (polyether modified polysiloxane wetting agent) of 0.3wt% of the total mass of the slurry are added. The configured slurry is applied on the PE base film by spraying, and the coating thickness is controlled to be 2μm, and double-sided coating is performed.
[0082] To ensure data credibility, three cells were assembled in parallel and numbered as Examples 4.1 to 4.3.
[0083] Battery test instructions:
[0084] The peel strength of the separator is measured according to the method in standard T / CPPIA10-2021.
[0085] Soft-pack battery hot box test: According to the method given in the national standard GB / T31485, the soft-pack battery cells that have been hot pressed are divided into different volumes and placed in a hot box. The temperature is gradually increased at a rate of 5°C / min and kept at the set temperature for 30 minutes. During this period, observe whether there is a fire and voltage changes. For the battery cells that have not caught fire or whose voltage has not dropped significantly, the temperature is increased by 10°C after 30 minutes and kept for 30 minutes, and the changes in the battery cells are continued to be observed. The temperature of the first insulation stage is 120°C.
[0086] Determination of battery capacity retention rate: At 25°C, charge the lithium-ion battery to 4.2V at a constant current of 0.2C, then charge at a constant voltage of 4.2V to a current of 0.05C, leave for 5 minutes, discharge at 0.2C to 2.7V, and record the measured discharge capacity as the initial capacity C0. Repeat the above steps for the same battery, and record the battery discharge capacity C100 after 100 cycles at the same time. The battery capacity retention rate after the cycle is 100%×C100 / C0.
[0087] The performance of the composite PVDF coated diaphragms obtained in Examples 1 to 3, the composite PTFE coated diaphragms obtained in Example 4, the coated diaphragms in Comparative Examples 1 to 3, and the lithium ion batteries obtained in Examples 1 to 4 and Comparative Examples 1 to 3 were tested, and the test results are shown in Table 1.
[0088] The PVDF and LLZO composite coating obtained in Example 1 was detected using a scanning electron microscope, and the SEM image was obtained as shown in FIG. Figure 1 As shown, the regular small balls are PVDF particles. It can be found that the PVDF particles in some areas have been deformed and fused together, indicating that the introduced LLZO can reduce the crystallinity of PVDF, thereby improving the liquid retention capacity of the diaphragm and improving the various mechanical properties of the diaphragm.
[0089] Table 1 Performance test results of diaphragm and lithium-ion battery
[0090]
[0091]
[0092] Compared with Comparative Example 1, the PVDF and LLZO composite coating applied in Example 1 will reduce the air permeability of the diaphragm, but the reduction is small and will not significantly affect the performance of the battery cell. Compared with Comparative Example 1 using a pure PE diaphragm, the capacity retention rate after 100 cycles is slightly higher. Compared with the LLZO solid electrolyte layer coated in Comparative Example 2, PVDF can effectively bond inorganic particles and significantly improve the peel strength of the coating. Compared with Comparative Example 1, both Examples 1 and Comparative Example 2 containing solid electrolyte coatings show better cycle stability, indicating that the lithium solid electrolyte coating can effectively improve the wettability and liquid retention rate of the electrolyte and maintain cycle stability. In addition, the precipitation of lithium ions in the solid electrolyte into the electrolyte can replenish lithium and thus increase the cycle capacity.
[0093] The hot box test detects the safety performance of the battery cell. There are two main reasons that may cause the battery cell to catch fire. First, the electrolyte gasifies severely at high temperature, and a strong chain reaction will occur when encountering an oxidant, leading to thermal runaway; second, the melting temperature of the PE diaphragm is 130-135°C. High temperature causes the diaphragm to melt, and the positive and negative electrodes short-circuit and release heat rapidly. The present invention can significantly improve the safety performance of the battery cell through the composite coating. The TEP in the coating increases the ignition temperature by 30°C through the flame retardant effect. In addition, the solid electrolyte particles remaining after the PE base film of the diaphragm shown in Comparative Example 2 melts can prevent the positive and negative electrodes from short-circuiting, and increase the temperature of the battery cell ignition and short circuit. However, the solid electrolyte particles cannot effectively isolate the positive and negative electrodes after losing the support of the base film. By introducing high-temperature resistant PVDF, its integrity can be enhanced and the temperature of short circuit can be increased.
[0094] Example 4 shows that this method is also applicable to other similar materials and has a positive impact on battery safety and cycle stability.
[0095] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A modified diaphragm having flame retardancy and strong mechanical properties, characterized in that: include: A base film and a coating disposed on at least one surface of the base film; The coating comprises a polymer, a phosphate flame retardant, a solid electrolyte, a wetting agent and a binder.
2. The modified diaphragm according to claim 1, characterized in that: The mass ratio of the polymer to the solid electrolyte is 1:(3-5).
3. The modified diaphragm according to claim 1, characterized in that: The coating is formed by slurry; the mass ratio of the polymer to the phosphate flame retardant in the slurry is 1:(11-15); The mass of the wetting agent is 0.3% to 0.5% of the mass of the slurry; The mass of the binder is 3% to 5% of the mass of the solid electrolyte.
4. The modified diaphragm according to claim 1, characterized in that: The polymer is selected from one or more of vinylidene fluoride-chlorotrifluoroethylene copolymer, polyvinyl fluoride, polyvinylidene fluoride, ethylene-chlorotrifluoroethylene copolymer, tetrafluoroethylene-hexafluoropropylene copolymer, ethylene-tetrafluoroethylene copolymer and tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer; The phosphate flame retardant is selected from one or more of trimethyl phosphate, triethyl phosphate, tri(2,2,2-trifluoroethyl) phosphate, tri(1,3-dichloro-2-propyl) phosphate, diphenyl cresol phosphate and diphenyl monooctyl phosphate; The solid electrolyte is selected from a lithium solid electrolyte or a sodium solid electrolyte; The lithium solid electrolyte is selected from one or more of a lithium lanthanum zirconium oxide solid electrolyte, a lithium lanthanum titanium oxide solid electrolyte and a lithium aluminum titanium phosphate solid electrolyte; The sodium solid electrolyte is selected from Na3AlF6, Na3ZrF6, Na2SiF6, Na 12 Al 12 Si 12 O 48 , NZSP and Na-β / β”-Al2O3; The wetting agent is one or more of an acetylenediol wetting agent and a polyether siloxane wetting agent; The binder is selected from one or more of carboxymethyl acrylate, sodium carboxymethyl cellulose, polyacrylamide-based binders, polyvinyl alcohol-based binders, and PVDF-based binders.
5. The modified diaphragm according to claim 1, characterized in that: The coating has a thickness of 1 to 5 μm.
6. The modified diaphragm according to claim 1, characterized in that: The base film is selected from polypropylene film or polyethylene film; the particle size of the solid electrolyte is 500-600nm.
7. A method for preparing a modified diaphragm having flame retardancy and strong mechanical properties as claimed in any one of claims 1 to 6, characterized in that: The following steps are involved: Coating the slurry on at least one surface of the base membrane to obtain a modified diaphragm; The slurry comprises a polymer, a phosphate flame retardant, a solid electrolyte, a wetting agent and a binder.
8. The preparation method according to claim 7, characterized in that: The slurry was prepared according to the following method: S1) mixing the solid electrolyte with a portion of the phosphate flame retardant to obtain slurry A; The polymer is mixed with the remaining phosphate flame retardant to obtain slurry B; S2) mixing the slurry A, slurry B, a wetting agent and a binder to obtain a slurry.
9. The preparation method according to claim 8, characterized in that: The solid content of the slurry A is 50% to 60%; the mass ratio of the polymer to the remaining phosphate flame retardant in the slurry B is 1:(8 to 10).
10. A secondary battery, characterized in that: It comprises the modified diaphragm with flame retardancy and strong mechanical properties as described in any one of claims 1 to 6 or the modified diaphragm with flame retardancy and strong mechanical properties prepared by the preparation method of any one of claims 7 to 9, a positive electrode and a negative electrode.
Citation Information
Patent Citations
Conductive ceramic composite diaphragm and solid-state battery
CN108878751A
Flame-retardant composite diaphragm, preparation method thereof and secondary battery
CN115832619A
High-performance surface-coated diaphragm of lithium power battery as well as preparation method and application of high-performance surface-coated diaphragm
CN116154403A
Separator for electrochemical device and electrochemical device including the same
CN118077093A