Infrared organic detector, array and chip
By using multi-layer electron transport layers and hole transport layers combined with infrared absorbing compounds in infrared organic detectors, the problem of insufficient detection capabilities of existing technologies in the band exceeding 1000nm is solved, and efficient short-wave infrared light detection is achieved, reducing the cost Dark current promotes the development and application of OPD.
Patent Information
- Application Number
- CN202410937625.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-10-29
AI Technical Summary
It is difficult for existing photodetectors to achieve high-performance detection in the infrared band range exceeding 1000nm, especially because silicon-based photodetectors cannot meet this demand, and the high cost of InGaAs-based photodetectors hinders their market application.
An infrared organic detector is designed, which adopts a structure including a first electrode, a photosensitive layer and a second electrode. The photosensitive layer uses an infrared absorbing compound with an absorption edge between 900nm and 2000nm, and is passed through a multi-layer electron transport layer and The hole transport layer improves photoelectric conversion efficiency and reduces dark current.
It significantly broadens the absorption spectrum of infrared organic detectors, improves the detection capability of short-wave infrared light, reduces dark current, and promotes the development and commercial application of OPD in the short-wave infrared region.
Smart Images

Figure CN118870831A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of organic photoelectric detectors, and more specifically, to an infrared organic detector, an array and a chip. Background Art
[0002] Photodetectors play a very important role in the development of modern society and have received widespread attention from academia and industry. At present, most of the photodetectors that have been successfully commercialized and widely used are inorganic photodetectors, such as silicon detectors and indium gallium arsenide detectors. However, silicon-based photodetectors cannot meet the detection requirements for infrared bands exceeding 1000nm. Image sensors based on InGaAs photodetectors, although they can meet the detection requirements in the short-wave infrared (SWIR) band (900-1700nm), are very expensive because they need to use a flip-chip bonding process to connect to the silicon-based readout circuit, which hinders their large-scale application in the market.
[0003] As an alternative material, organic semiconductor materials have the advantages of high absorption coefficient, adjustable energy level and absorption spectrum, flexibility, light weight, and large-area solution processing, making them easy to integrate into CMOS or thin-film transistor (TFT) backplanes, providing new opportunities for wearable electronic devices and artificial intelligence. With the development of organic semiconductor materials, organic photodetectors (OPDs) have shown excellent light detection performance in the 1000nm band. However, in the band range exceeding 1000nm, the development of OPDs is still greatly restricted due to the constraints of the characteristics of organic semiconductor materials.
[0004] Therefore, finding an infrared detector that can detect infrared bands above 1000nm and achieve high performance is a problem we need to solve. Summary of the invention
[0005] The purpose of the present invention is to disclose an infrared organic detector, array and chip. The organic photodetector has extremely high responsiveness and extremely low dark current in the infrared band region exceeding 1000nm, which can greatly improve the organic photodetector's ability to detect weak light in the infrared band region exceeding 1000nm.
[0006] The technical solution adopted by the present invention is:
[0007] An infrared organic detector, the infrared organic detector comprising a first electrode, a second electrode, and a
[0008] A photosensitive layer, a charge transport layer disposed between the first electrode and the photosensitive layer and / or between the second electrode and the photosensitive layer;
[0009] Wherein, the photosensitive layer comprises an infrared absorbing compound, and the absorption edge of the infrared absorbing compound is between 900nm and 2000nm.
[0010] The first electrode and the second electrode may be formed of any conductive material.
[0011] If we list examples of the constituent materials of the electrodes (first electrode, second electrode), we can cite: metals such as platinum, gold, silver, aluminum, chromium, nickel, copper, titanium, magnesium, calcium, barium, sodium, or their alloys; metal oxides such as indium oxide and tin oxide, or their composite oxides (such as ITO, IZO); conductive polymers such as polyaniline, polypyrrole, polythiophene, polyacetylene, etc.; those obtained by adding dopants such as hydrochloric acid, sulfuric acid, sulfonic acid, Lewis acids such as FeCl3, halogen atoms such as iodine, metal atoms such as sodium, potassium, etc. to the above conductive polymers; conductive composite materials in which conductive particles such as metal particles, carbon black, fullerene, carbon nanotubes, etc. are dispersed in a matrix such as a polymer binder, etc. The constituent materials of the electrodes can be used alone or in combination of two or more in any combination and ratio.
[0012] Examples of transparent electrode materials include composite oxides such as indium tin oxide (ITO) and indium zinc oxide (IZO); and metal thin films.
[0013] When the first electrode is close to the side of the incident light and the second electrode is far away from the side of the incident light.
[0014] Preferably, the second electrode may be formed of a conductive metal material (e.g., an electrically conductive metal material, a thermally conductive metal material, a combination thereof, etc.). For example, the second electrode may be formed of a metal such as magnesium (Mg), aluminum (Al), scandium (Sc), titanium (Ti), vanadium (V), chromium (Cr), manganese (Mn), nickel (Ni), copper (Cu), zinc (Zn), gallium (Ga), zirconium (Zr), niobium (Nb), molybdenum (Mo), lead (Pb), silver (Ag), cadmium (Cd), indium (In), tin (Sn), lanthanum (La), hafnium (Hf), tantalum (Ta), tungsten (W), iridium (Ir), platinum (Pt), gold (Au) or bismuth (Bi) or an alloy thereof.
[0015] Preferably, the first electrode may be formed of a transparent conductive material (may at least partially include a transparent conductive material), so that the first electrode may be configured to allow light to pass through and satisfy a transmittance greater than 60%. For example, the first electrode may be formed of a transparent conductive oxide such as ITO, IZO or ZnO, or graphene. The transmittance may generally be measured by a spectrophotometer.
[0016] Preferably, the electrodes (first electrode, second electrode) have the function of capturing holes and electrons generated in the photosensitive layer. Therefore, as the constituent material of the electrode, among the above materials, it is preferred to use constituent materials suitable for capturing holes and electrons. If electrode materials suitable for capturing holes are listed, for example, materials with high work functions such as Au and ITO can be cited. If electrode materials suitable for capturing electrons are listed, for example, materials with low work functions such as Al can be cited.
[0017] In this embodiment, there is no limitation on the method for forming the electrode. The electrode can be formed, for example, by one or more dry processes selected from solution film formation, sol-gel film formation, vacuum thermal evaporation, atomic layer deposition, chemical vapor deposition, electrodeposition, and anodization. In addition, for example, it can also be formed by a wet process using conductive ink or the like. In this case, any conductive ink can be used as the conductive ink, for example, a conductive polymer, a metal particle dispersion, etc. can be used.
[0018] Preferably, when the first electrode is a cathode, the charge transport layer between the first electrode and the photosensitive layer is an electron transport layer, and the electron transport layer includes an N-type material;
[0019] The corresponding second electrode is an anode, and the charge transport layer between the second electrode and the photosensitive layer is a hole transport layer, which includes a P-type material.
[0020] Further, when the first electrode is an anode, the charge transport layer between the first electrode and the photosensitive layer is a hole transport layer, and the hole transport layer includes a P-type material;
[0021] The corresponding second electrode is a cathode, and the charge transport layer between the second electrode and the photosensitive layer is an electron transport layer, which includes an N-type material.
[0022] Preferably, the charge transport layer includes at least two charge transport sublayers, that is, the electron transport layer includes at least two electron transport sublayers, and the hole transport layer includes at least two hole transport sublayers.
[0023] The electron transport layer of the present invention is provided with at least two electron transport sublayers, which can improve the photoelectric conversion efficiency and reduce the dark current.
[0024] Therefore, the LUMO difference between the electron transport sublayer and the n-type semiconductor of the photosensitive layer is preferably 1.5 eV or less, preferably 1.0 eV.
[0025] When reducing dark current by the electron transport sublayer, the electron transport sublayer preferably has a HOMO deeper than 0.3 eV, preferably has a HOMO deeper than 0.5 eV, and further preferably has a HOMO deeper than 1.0 eV relative to the p-type semiconductor of the photosensitive layer.
[0026] The material of the electron transport sublayer is selected from organic compound 1, inorganic compound 1, or a combination thereof; wherein the organic compound 1 is selected from fullerene and its derivatives, 4,7-diphenyl-1,10-phenanthroline, polyethyleneimine, polyethoxyethyleneimine, 2,9-dimethyl-4,7-biphenyl-1,10-phenanthroline, [9,9-dioctylfluorene-9,9-bis(N,N-dimethylaminopropyl)fluorene], bromo-[9,9-dioctylfluorene-9,9-bis(N,N-dimethylaminopropyl)fluorene] 1,3,5-tris(1-phenyl-1H-benzimidazol-2-yl)benzene, bis(2-methyl-8-quinoline)-4-(phenylphenol)aluminum, 1,3,5-tris[(3-pyridyl)-phenyl-3-yl]benzene, or a mixture or composite of the above materials; the inorganic compound 1 is selected from zinc oxide, tin oxide, aluminum-doped zinc oxide, magnesium-doped zinc oxide, gallium-doped zinc oxide, titanium oxide, tantalum oxide, zinc sulfide, chromium sulfide, or a mixture or composite of the above materials. The film thickness of the electron transport layer is usually 1 nm or more, preferably 5 nm or more and usually 300 nm or less, preferably 100 nm or less.
[0027] The material of the hole transport sublayer is selected from organic compound 2, inorganic compound 2, or a combination thereof; wherein the organic compound 2 is selected from 4,4'-cyclohexylbis[N,N'-bis(4-methylphenyl)aniline], N,N'-bis(naphthalene-1-yl)-N,N'-bis(phenyl)-benzidine, N,N'-bis(naphthalene-1-yl)-N,N'-bis(phenyl)-2,7-diamino-9,9-spirobifluorene, 2,2',7, One or more of 7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene, 4,4',4"-tri(carbazole-9-yl)triphenylamine, poly(4-butyltriphenylamine), polyvinylcarbazole, polystyrene-N,N'-diphenyl-N,N'-bis-(3-methylphenyl)-(1,1)-biphenyl-4,4'-diamineperfluorocyclobutane, poly(3,4-ethylenedioxythiophene) mixed polystyrene sulfonate;
[0028] The inorganic compound 2 is selected from tungsten oxide, molybdenum oxide, vanadium oxide, chromium oxide, nickel oxide, copper oxide, cuprous oxide, cuprous thiocyanate, copper sulfide, copper iodide, or a mixture or a composite of the above materials.
[0029] The preparation of the electron transport layer and the hole transport layer are independently selected from one or more of solution film formation, sol-gel film formation, vacuum thermal evaporation, atomic layer deposition, chemical vapor deposition, electrodeposition, and anodization.
[0030] Further, when the charge transport layer is an electron transport layer, the LUMO energy level difference between two adjacent transport sublayers is less than or equal to 1.0 eV.
[0031] Further, when the charge transport layer is a hole transport layer, the HOMO energy level difference between two adjacent transport sublayers is less than or equal to 1.0 eV.
[0032] When the LUMO energy level difference between two adjacent transport sublayers is less than or equal to 1.0 eV, it is beneficial for electrons to transfer between two adjacent transport sublayers. When the HOMO energy level difference between two adjacent transport sublayers is less than or equal to 1.0 eV, it is beneficial for holes to transfer between two adjacent transport sublayers.
[0033] The infrared organic detector of the present invention can be formed by stacking a first electrode, a hole transport layer, a photosensitive layer, an electron transport layer and a second electrode in order, but usually a substrate is provided to support these layers. The substrate can be arranged on either the first electrode side or the second electrode side, or on both sides. The substrate is preferably arranged at least on the first electrode side.
[0034] The substrate may be formed of any material, but when light is incident from the substrate side, it needs to be formed of a material with high transparency.
[0035] If we list examples of the constituent materials of the substrate, we can cite: inorganic materials such as glass, sapphire, and titanium dioxide; organic materials such as polyethylene terephthalate, polyethylene naphthalate, polyethersulfone, polyimide, nylon, polystyrene, polyvinyl alcohol, ethylene-vinyl alcohol copolymer, fluororesin, vinyl chloride, polyethylene, cellulose, polyvinylidene chloride, aromatic polyamide, polyphenylene sulfide, polyurethane, polycarbonate, polyarylate, and polynorbornene; paper materials such as paper and synthetic paper; composite materials such as materials obtained by coating or laminating metals such as stainless steel, titanium, and aluminum with insulating properties, etc. The constituent materials of the substrate may be used alone or in combination of two or more in any combination and ratio.
[0036] The shape and size of the substrate are not limited and can be set arbitrarily. If the thickness of the substrate is too thin, the strength is insufficient and it cannot fulfill the function as a supporting member. If it is too thick, the cost increases. The substrate is usually in the form of a film or plate of about 10μm to 50mm.
[0037] In order to impart gas barrier properties and control the surface state, other layers may be stacked on the substrate.
[0038] The infrared absorbing compound includes an N-type receptor material of the following structural formula:
[0039]
[0040] In formula (I), n represents the number of repeating units of the polymer. When n is 1, the copolymerization unit in formula (I) does not exist; when n is a natural number between 2 and 10,000, the copolymerization unit in formula (I) exists; A is an electron withdrawing group; B is a π bridge; C and the copolymerization unit are both conjugated aromatic ring units.
[0041] Furthermore, the A unit is selected from any one of the following structures:
[0042]
[0043] Wherein, dotted line ① represents the connection site between the copolymer unit and the A unit, and dotted line ② represents the connection site between the B unit and the A unit; X1 is independently selected from hydrogen, halogen, trifluoromethyl, cyano, nitro, C1-C30 straight chain, branched or cyclic alkyl, C1-C30 straight chain, branched or cyclic alkoxy, C1-C30 straight chain, branched or cyclic alkylthio;
[0044] Any one or more hydrogen atoms in the A unit are not substituted by other atoms and / or groups, or are independently substituted by protium, deuterium or tritium atoms.
[0045] Further, the B units are each independently selected from the formula The group shown, or The group shown, or The group shown, or The groups shown, or not present;
[0046] wherein R1 is independently selected from one or more of a hydrogen atom, a halogen, an ester group, a hydroxyl group, a nitro group, a cyano group, an alkyl group, an alkyl derivative, an alkylene group, an alkylene derivative, an aralkyl group, and an aralkyl derivative;
[0047] One or more carbon atoms on the alkyl derivative, alkylene derivative or aralkyl derivative are substituted by one or more of oxygen atoms, amino groups, sulfone groups, carbonyl groups, aryl groups, olefin groups, alkynyl groups, ester groups, cyano groups and nitro groups;
[0048] and / or
[0049] One or more hydrogen groups on the alkyl derivative, alkylene derivative or aralkyl derivative are replaced by one or more of halogen, hydroxyl, amino, carboxyl, cyano, nitro, aryl, alkene or alkyne groups;
[0050] Y1 is independently selected from O, S, Se or N-R1;
[0051] Any one or more hydrogen atoms in the B unit are not substituted by other atoms and / or groups, or are independently substituted by protium, deuterium or tritium atoms.
[0052] Further, the C unit is selected from any one of the following structures:
[0053]
[0054] wherein R2 is independently selected from one or more of hydrogen, halogen, ester, hydroxyl, nitro, cyano, alkyl, alkyl derivative, alkylene, alkylene derivative, aralkyl, aralkyl derivative; or is absent;
[0055] One or more carbon atoms on the alkyl derivative, alkylene derivative or aralkyl derivative are substituted by one or more of oxygen atoms, amino groups, sulfone groups, carbonyl groups, aryl groups, olefin groups, alkynyl groups, ester groups, cyano groups and nitro groups;
[0056] and / or
[0057] One or more hydrogen groups on the alkyl derivative, alkylene derivative or aralkyl derivative are replaced by one or more of halogen, hydroxyl, amino, carboxyl, cyano, nitro, aryl, alkene or alkyne groups;
[0058] Y2 is independently selected from O, S, Se or N-R1;
[0059] Z1 is each independently selected from N, C, Si or Ge;
[0060] Any one or more hydrogen atoms in the C unit are not substituted by other atoms and / or groups, or are independently substituted by protium, deuterium or tritium atoms.
[0061] Furthermore, the copolymerization unit is selected from any one of the following structural formulas and combinations thereof:
[0062]
[0063] Wherein, R3 is independently selected from hydrogen, halogen, trifluoromethyl, cyano, nitro, C1-C60 straight chain, branched or cyclic alkyl, C1-C60 straight chain, branched or cyclic alkoxy, C1-C60 straight chain, branched or cyclic alkylthio, alkyl substituted aryl; the alkyl in the alkyl substituted aryl is a straight chain or branched alkyl with 1 to 60 carbon atoms, and the aryl is a benzene ring or a thiophene ring;
[0064] Y3 is independently selected from O, S, Se or N-R1;
[0065] Z2 is each independently selected from N, C, Si or Ge;
[0066] Any one or more hydrogen atoms in the copolymerized units are not substituted by other atoms and / or groups, or are independently substituted by protium, deuterium or tritium atoms.
[0067] The specific molecular structure of the structural formula (I) of the present invention may be, but is not limited to, any of the following structures:
[0068]
[0069] wherein R is independently selected from one or more of a hydrogen atom, a halogen, an ester group, a hydroxyl group, a nitro group, a cyano group, an alkyl group, an alkyl derivative, an alkylene group, an alkylene derivative, an aralkyl group, and an aralkyl derivative;
[0070] One or more carbon atoms on the alkyl derivative, alkylene derivative or aralkyl derivative are substituted by one or more of oxygen atoms, amino groups, sulfone groups, carbonyl groups, aryl groups, olefin groups, alkynyl groups, ester groups, cyano groups and nitro groups;
[0071] and / or
[0072] One or more hydrogen groups on the alkyl derivative or alkylene derivative or aralkyl derivative are substituted by one or more of halogen, hydroxyl, amino, carboxyl, cyano, nitro, aryl, alkene, and alkyne groups.
[0073] An infrared organic detector array comprises a plurality of picture elements, and the picture elements comprise the infrared organic detectors.
[0074] Preferably, the infrared organic detector array further comprises a substrate; the substrate comprises a pixel readout circuit composed of a silicon-based complementary metal oxide semiconductor transistor or a thin film transistor.
[0075] An infrared organic detector chip comprises the infrared organic detector array.
[0076] Compared with the prior art, the present invention has the following beneficial effects:
[0077] Based on this, the present invention designs a photosensitive layer of an infrared organic detector including an infrared absorbing compound with an absorption edge between 900nm and 2000nm, broadens the absorption spectrum of the infrared organic detector to 2000nm, greatly improves the detection wavelength and photoelectric response range of the OPD device, has good device performance in the short-wave infrared region, and has important research significance and a wide range of application scenarios in OPD and other optoelectronic fields. The present invention can greatly improve the detection capability of the infrared organic detector for short-wave infrared light through device engineering and interface regulation, and has played a great role in promoting the development and commercial application of short-wave infrared OPDs. BRIEF DESCRIPTION OF THE DRAWINGS
[0078] Figure 1 This is a schematic diagram of the structure of an infrared organic detector provided in Example 1.
[0079] Figure 2This is a schematic diagram of the structure of another infrared organic detector provided in Example 1.
[0080] Figure 3 This is a schematic diagram of the structure of another infrared organic detector provided in Example 1.
[0081] Figure 4 This is a schematic diagram of the structure of an infrared organic detector with a multi-layer transmission layer provided in Example 1.
[0082] Figure 5 This is a schematic diagram of the structure of an infrared organic detector with a multi-layer electron transport layer provided in Example 1.
[0083] Figure 6 This is a schematic diagram of the structure of an infrared organic detector with a multi-layer hole transport layer provided in Example 1.
[0084] Figure 7 It is the ultraviolet-visible absorption spectrum of the infrared organic detector prepared in Examples 6 and 9.
[0085] Figure 8 It is the dark current diagram of the infrared organic detector prepared in Examples 6, 7 and 8.
[0086] Fig. 9 It is the EQE diagram of the infrared organic detector prepared in Examples 6, 7 and 8.
[0087] Fig.10 It is the responsivity diagram of the infrared organic detectors prepared in Examples 6, 7 and 8.
[0088] Fig.11 This is a graph of the relative detectivity of the infrared organic detectors prepared in Examples 6, 7, and 8.
[0089] Fig.12 This is a cross-sectional view of an infrared organic detector array provided in Example 10.
[0090] Fig.13 This is a top view of an infrared organic detector array provided in Example 10.
[0091] Fig.14 It is a schematic diagram of using a detector chip to detect an object to be detected.
[0092] Fig.15 This is an example of imaging the object under test using a visible light detector.
[0093] Fig.16 This is an imaging example of using an infrared organic detector to detect the object to be tested.
[0094] In the figure: 1-first electrode, 2-electron transport layer, 201-electron transport sublayer, 3-photosensitive layer, 4-hole transport layer, 401-hole transport sublayer, 5-second electrode, 6-pixel, 7-packaging layer, 8-pixel readout circuit, 9-substrate, 10-infrared organic detector array. DETAILED DESCRIPTION
[0095] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. The present invention is described in detail below in combination with the drawings and specific implementation methods.
[0096] It should be understood that when used in this specification and the appended claims, the terms "include" and "comprises" indicate the presence of described features, integers, steps, operations, elements and / or components, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components and / or combinations thereof.
[0097] It should also be understood that the terms used in this specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. As used in the specification of the present invention and the appended claims, unless the context clearly indicates otherwise, the singular forms "a", "an" and "the" are intended to include plural forms.
[0098] It should be further understood that the term "and / or" used in the present description and the appended claims refers to and includes any and all possible combinations of one or more of the associated listed items.
[0099] Example 1
[0100] This embodiment provides an infrared organic detector, taking the first electrode 1 as a cathode and the second electrode 5 as an anode as an example, the infrared organic detector includes a cathode, an anode, a photosensitive layer 3 arranged between the cathode and the anode, an electron transport layer 2 arranged between the cathode and the photosensitive layer 3, and a hole transport layer 4 between the anode and the photosensitive layer; Figure 1 shown.
[0101] In this embodiment, the main function of the electron transport layer 2 is to transfer the electrons generated by the photosensitive layer 3 under light excitation to the cathode, blocking the holes from moving in the direction of electron movement, thereby effectively transmitting electrons, improving the photoelectric conversion efficiency, and reducing dark current.
[0102] Similarly, the main function of the hole transport layer 4 is to transfer the holes generated by the photosensitive layer under light excitation to the anode and block the electrons from moving in the direction of the holes, thereby effectively transporting holes, improving the photoelectric conversion efficiency and reducing the dark current.
[0103] The structure of the infrared organic detector can also be Figure 2 The structure shown specifically includes a cathode, an anode, a photosensitive layer 3 arranged between the cathode and the anode, and an electron transport layer 2 arranged between the cathode and the photosensitive layer 3.
[0104] The structure of the infrared organic detector can also be Figure 3 The structure shown specifically includes a cathode, an anode, a photosensitive layer 3 disposed between the cathode and the anode, and a hole transport layer 4 between the anode and the photosensitive layer.
[0105] In a specific embodiment, the hole transport layer 4 may also include two or more hole transport sublayers 401; similarly, the electron transport layer 2 includes two or more electron transport sublayers 201. The specific detector structure is as follows: Figure 4 , Figure 5 , Figure 6 shown. Figure 4 , Figure 5 , Figure 6 These are just a few cases listed. As long as the infrared organic detector includes one or more electron transport layers and one or more hole transport layers; or the infrared organic detector has only one or more electron transport layers; or the infrared organic detector has only one or more hole transport layers; they all fall within the protection scope of the present invention.
[0106] The LUMO energy level difference between two adjacent electron transport sublayers 201 in the electron transport layer 2 is less than or equal to 1.0 eV. The HOMO energy level difference between two adjacent hole transport sublayers 401 in the hole transport layer 4 is less than or equal to 1.0 eV.
[0107] In this embodiment, since a smaller LUMO energy level difference is more conducive to the transmission of electrons, more electrons can be transferred to the cathode through the above arrangement. Similarly, since a smaller HOMO energy level difference is more conducive to the transmission of holes, more holes can be transferred to the anode through the above arrangement.
[0108] Figure 1 to Figure 6 The photosensitive layer 3 in the infrared organic detector includes an infrared absorbing compound, and the absorption edge of the infrared absorbing compound is between 900nm and 2000nm.
[0109] Since the photosensitive layer 3 of the infrared organic detector provided in this embodiment includes an infrared absorbing compound with an absorption edge between 900nm and 2000nm, the infrared organic detector can detect infrared rays exceeding the 1000nm band. In addition, this embodiment can effectively reduce dark current by providing an electron transport layer and a hole transport layer, especially a multi-layer electron transport layer and a multi-layer hole transport layer.
[0110] Example 2
[0111] This embodiment provides a method for synthesizing an N-type acceptor material, wherein the N-type acceptor material is used as an infrared absorbing compound in a photosensitive layer.
[0112] Specifically provide the synthesis of brominated N-type acceptor materials containing fluoroquinone end groups:
[0113] The specific reaction steps and reaction conditions are as follows:
[0114]
[0115] Synthesis of compound 2:
[0116] Compound 1 (20 g) was added to a 1000 ml two-necked reaction bottle, and 400 ml of glacial acetic acid was added, stirred thoroughly, and an aqueous solution (40 ml) of chromium trioxide (18 g) was added dropwise. The reaction mixture was reacted in an oil bath at 100 ° C for two hours. After the detection reaction was completed, the reaction mixture was cooled to room temperature and then extracted three times with ethyl acetate. The organic layer was collected, dried over anhydrous sodium sulfate, filtered, and concentrated under reduced pressure to obtain a crude product. It was then further purified by silica gel column chromatography to obtain compound 2 (5.12 g, 23.4%) as a yellow solid. 1 H NMR (400MHz, CDCl3) δ8.26 (d, 1H), 7.83 (s, 1H).
[0117] Synthesis of compound 3:
[0118] Compound 2 (5 g) and malononitrile (1.4 g) were added to a 100 ml two-necked bottle. After three times of ventilation, the reaction system was placed in an inert atmosphere, 50 ml of ultra-dry dichloromethane was added, and a solution of titanium tetrachloride in dichloromethane (1M, 21.3 ml) was added dropwise at 0°C. After the reaction mixture was stirred at 0°C for 1.5 hours, anhydrous pyridine (1.7 g) was added dropwise, and the reaction was continued for 2 hours under this condition. After the detection reaction was completed, the reaction mixture was poured into water and then extracted three times with ethyl acetate. The organic layer was collected, dried over anhydrous sodium sulfate, filtered, and concentrated under reduced pressure to obtain a crude product. It was then further purified by silica gel column chromatography to obtain compound 3 (1.1 g, 19.4%) as a yellow solid. 1H NMR (400MHz, CDCl3) δ8.71(d,1H),8.42(s,1H).
[0119] Synthesis of compound 6:
[0120] The specific reaction steps and reaction conditions are as follows:
[0121]
[0122] Synthesis of compound 5:
[0123] Compound 4 (0.8 g) was added to a 150 ml two-mouth reaction bottle, and the reaction system was ventilated three times to place the reaction system in an inert atmosphere, and 50 ml of ultra-dry tetrahydrofuran was added. After the reaction system was cooled to -78 ° C, lithium diisopropylamide (0.5M, 12.24 ml) was added dropwise. After the addition was complete, the reaction mixture was allowed to react at -78 ° C for 1 hour, and then tributyltin chloride (0.7 g) was added, and the mixture was heated to room temperature and stirred for 3 hours. The reaction mixture was poured into water and extracted three times with dichloromethane. The organic layer was collected, dried over anhydrous sodium sulfate, filtered, and concentrated under reduced pressure to obtain compound 5 (crude product), which was used directly in the next step without further purification.
[0124] Synthesis of compound 6:
[0125] Compound 5 (1 g) and compound 3 (0.75 g) and catalyst tetrakistriphenylphosphine palladium (0.05 g) were added to a 250 ml two-mouth reaction bottle, and the air was evacuated three times to make the reaction system in an inert atmosphere. After adding 120 ml of ultra-dry toluene, the reaction was carried out at 110 ° C for 5 hours. After the reaction was detected to be completed, the reaction solution was cooled to room temperature and poured into water, and then extracted with dichloromethane three times. The organic layer was collected, dried with anhydrous sodium sulfate, filtered, and concentrated under reduced pressure to obtain a crude product. It was further purified by silica gel column chromatography to obtain a dark solid compound 6 (0.31 g, 30.1%). 1 H NMR (400MHz, CDCl3) δ8.74(d,1H),8.21(s,1H),4.69(d,2H),3.41–2.81(m,2H),2.15–2.08(m,1H),2.07–1.96(m,2H),1.37–0.75(m,57H).
[0126] Example 3
[0127] Synthesis of P1:
[0128] The specific reaction steps and reaction conditions are as follows:
[0129]
[0130] Compound 6 (100 mg, 0.0514 mmol), polymer monomer 2,5-bis(trimethyltinyl)thiophene (21.1 mg, 0.0514 mmol), catalyst tri(dibenzylidene indene acetone) dipalladium (2 mg) and ligand tri-o-methylphenylphosphine (4 mg) were added to a 15 ml reaction bottle, ventilated three times through a double-row tube, and 5 mL of chlorobenzene was added with a syringe. The reaction solution was stirred at 120 ° C for 36 hours. After the reaction solution returned to room temperature, the reaction solution was added dropwise to 200 mL of methanol and filtered with filter paper to obtain a crude polymer product. The crude polymer product was extracted with methanol, n-hexane, dichloromethane, and chloroform in a Soxhlet extraction device, and the extracted chloroform phase was collected and concentrated and precipitated in methanol. The solid was collected by filtration and dried to obtain the target polymer P1, 80%.
[0131] Example 4
[0132] Synthesis of P2:
[0133] The specific reaction steps and reaction conditions are as follows:
[0134]
[0135] Compound 66 (100 mg, 0.0514 mmol), polymerizable monomer 2,5-bis(trimethyltinyl)selenophene (23.5 mg, 0.0514 mmol), catalyst tri(dibenzylideneacetone)dipalladium (2 mg) and ligand tri-o-methylphenylphosphine (4 mg) were added to a 15 ml reaction bottle, ventilated three times through a double-row tube, and 5 mL of chlorobenzene was added with a syringe. The reaction solution was stirred at 120 ° C for 36 hours. After the reaction solution returned to room temperature, the reaction solution was added dropwise to 200 mL of methanol and filtered with filter paper to obtain a crude polymer product. The crude polymer product was extracted with methanol, n-hexane, dichloromethane and chloroform in a Soxhlet extraction device, and the extracted chloroform phase was collected and concentrated and precipitated in methanol. The solid was collected by filtration and dried to obtain the target polymer P2, 83%.
[0136] Example 5
[0137] Table 1 below lists other N-type electron acceptor materials of this series, and their molecular structures are shown below. The preparation method is basically the same as that of Examples 2 to 4, except that the relevant monomers are replaced. Since the preparation method is similar, it will not be described in detail here.
[0138] Table 1
[0139]
[0140]
[0141]
[0142]
[0143] Example 6
[0144] The device structure of the organic photodetector used in this embodiment is as follows: Figure 1 As shown, from top to bottom are the first electrode 1 (cathode), the electron transport layer 2, the photosensitive layer 3, the hole transport layer 4, and the second electrode 5 (anode).
[0145] Among them, the cathode is made of indium tin oxide (ITO); the electron transport layer is made of zinc oxide; the hole transport layer is made of molybdenum oxide, and the anode is metallic silver.
[0146] The photosensitive layer 3 adopts a bulk heterojunction structure, which is composed of a blend of an electron donor material and an electron acceptor material. In fact, the photosensitive layer 3 can also adopt a planar heterojunction structure. The electron acceptor material can be selected from any one of the N-type organic materials P1 to P21 in Examples 3 to 5, and the corresponding electron donor material can be selected from any one of the following materials:
[0147]
[0148] The electron donor material in this embodiment is preferably NT812, and the corresponding electron donor material is the N-type organic material P1 in Example 6. The mass ratio of NT812 to P1 is 1:1.5.
[0149] The method for preparing the organic photodetector comprises the following steps:
[0150] S1. The ITO conductive substrate is ultrasonically treated and cleaned with isopropyl alcohol, detergent, deionized water, and acetone in sequence, with each treatment lasting 20 minutes. The cleaned ITO conductive substrate is then placed in an oven at 60°C and dried for 5 hours; the ITO conductive substrate is then subjected to plasma surface treatment;
[0151] S2. Dissolve 0.4 g zinc acetate in a mixed solvent of 4 ml 2-methoxyethanol and 110 μl ethanolamine, and then heat and stir at 50°C for 10 h to obtain a sol-gel zinc oxide precursor solution. Spin-coat the solution at 3300 rpm for 30 s, and anneal on a hot plate at 150°C for 30 min to obtain a 30 nm thick zinc oxide film.
[0152] S3. Blend the donor material NT812 and the acceptor material P1 in the above mass ratio and add them into a mixed solvent of chlorobenzene and 1-chloronaphthalene (98:2, v / v) to make the mass concentrations of NT812 and P1 10 mg / ml and 15 mg / ml respectively. Stir well for 3 hours at 65°C, then spin-coat on the zinc oxide film at a speed of 800 rpm for 1 minute, and thermally anneal at 100°C for 10 minutes to finally obtain a photosensitive layer film of a specified thickness.
[0153] S4. The above structure is transferred to a thermal evaporation device at 5×10 -7 Under vacuum conditions of torr, a molybdenum oxide film of a specified thickness is formed. The photosensitive layer is deposited on the above-mentioned photosensitive layer film by thermal evaporation at a rate of.
[0154] S5. In 5×10 -7 Under vacuum conditions of 0.1 torr, a silver film of a specified thickness was thermally evaporated on a molybdenum oxide film as an anode to obtain a highly sensitive organic photodiode.
[0155] Example 7
[0156] The device structure, materials used and device preparation method in this embodiment are basically the same as those in Example 6, and the only difference is the composition of the photosensitive layer. In this embodiment, the photosensitive layer introduces a third component Y6 to improve the device performance of the organic photodetector. The three components in the photosensitive layer are NT812:P1:Y6, and the mass ratio is 1:1.1:0.4.
[0157] Example 8
[0158] The device structure of the organic photodetector in this embodiment is as follows: Figure 4 As shown, from top to bottom are the first electrode 1 (cathode), the electron transport layer 2, the photosensitive layer 3, the hole transport layer 4, and the second electrode 5 (anode).
[0159] Among them, the cathode adopts indium tin oxide (ITO); in this embodiment, the electron transport layer includes two layers, namely zinc oxide and fullerene self-assembled layer C60-SAM, and zinc oxide is deposited first and then C60-SAM; the hole transport layer includes two layers, namely cuprous thiocyanate (CuSCN) and molybdenum oxide, and CuSCN is deposited first and then molybdenum oxide; the anode is metallic silver.
[0160] In this embodiment, except for the fullerene self-assembled layer C60-SAM and cuprous thiocyanate (CuSCN), the preparation methods of other layers are the same as those in Embodiment 6.
[0161] Preparation of C60-SAM: 1 mg of C60-SAM was dissolved in 1 mL of a mixed solvent of chloroform and tetrahydrofuran with a volume ratio of 1:1; then heated and stirred at 50°C for 2 h; it was spin-coated on a zinc oxide film at a speed of 3000 rpm for 30 s, and annealed on a hot stage at 100°C for 10 min.
[0162] Preparation of CuSCN: 20 mg of CuSCN was dissolved in 1 mL of ethyl sulfide, and then heated and stirred at 50°C for 2 h; it was spin-coated on the photosensitive layer at a speed of 3000 rpm for 30 s, and annealed on a hot stage at 100°C for 10 min.
[0163] Example 9
[0164] The device structure, materials used and device preparation method in this embodiment are basically the same as those in Embodiment 6, and the only difference is the composition of the photosensitive layer. In this embodiment, the N-type acceptor material in the photosensitive layer is P2.
[0165] Test Example 1
[0166] The photoelectric properties of the above-mentioned embodiments 6 to 9 were tested respectively by the method in the literature (DOI: 10.1063 / 5.0018274), including dark current, external quantum efficiency EQE, responsivity R and specific detection rate D*. Figure 7 to Figure 11 And as shown in Table 2.
[0167] Table 2. Dark current, EQE, responsivity, and specific detectivity of Examples 6-8 at 1000 nm
[0168]
[0169] Note: Dark current is the value at -0.1V bias.
[0170] By comparing with the above-mentioned method in which a single-layer transmission layer is used and P1 is used as the photosensitive layer, it is not difficult to see that after using two transmission sublayers, the EQE of the corresponding infrared organic detector is significantly increased after 900nm, and is above 40%; at the same time, it has a higher specific detection rate in the short-wave infrared region, which greatly improves the detection ability of the photodetector for short-wave infrared light. Therefore, the infrared organic detector corresponding to the two transmission sublayers preferably has a more balanced carrier mobility, lower dark current and higher EQE response.
[0171] Example 10
[0172] Based on the infrared organic detectors provided in the above embodiments, this embodiment also provides an infrared organic detector array, wherein the infrared organic detector array 10 includes a plurality of pixels 6, and the pixel 6 includes the infrared organic detector as described in Embodiment 1. The specific structure of the infrared organic detector can adopt a structure in Embodiment 1.
[0173] The photosensitive layer of the infrared organic detector includes an infrared absorbing compound, and the absorption edge of the infrared absorbing compound is between 900nm and 2000nm. Preferably, the infrared absorbing compound in the photosensitive layer 3 is preferably any one of the N-type organic materials P1 to P21 in the above embodiments.
[0174] In this embodiment, the infrared organic detector array 10 further includes a substrate 9; the substrate 9 includes a pixel readout circuit 8 composed of a silicon-based complementary metal oxide semiconductor transistor or a thin film transistor.
[0175] In a specific embodiment, based on Figure 4 The infrared organic detector array 10 is composed of the infrared organic detector (the electron transport layer 2 is two layers of electron transport sublayers 201, and the hole transport layer 4 is two layers of hole transport sublayers 401). The device structure of the infrared organic detector array 10 is as follows Fig.12 , Fig.13 As shown in the figure, it can be seen that the infrared organic detector array 10 includes, from bottom to top, a pixel readout circuit 9 made on a single crystal silicon substrate and composed of silicon-based complementary metal oxide semiconductor transistors (MOSFETs), and each pixel readout circuit is linked to a first electrode 1 (cathode here) array that defines the pixel size. Above the cathode array are the electron transport layer 2, the photosensitive layer 3, the hole transport layer 4, the second electrode 5 (anode here) and the encapsulation layer 7. From the electron transport layer 2, the photosensitive layer 3, the hole transport layer 4, the second electrode 5 to the encapsulation layer 7, they are all continuous structures in the entire array area, and no patterning processing is required between the pixels 6.
[0176] It should be noted that in the array device, when the incident light is incident from the anode, if the anode is made of silver, its thickness is less than 30 nm, or it is made of other transparent materials to ensure the transparency of the anode.
[0177] The array is composed of N×M pixels, the size of the pixel 6 is 25 μm, the number of pixels is 1×256 or 1×512, and imaging tests are carried out on it. The results show that Fig.13 The infrared organic detector array in which the pixels are defined by the bottom electrode (ie, the first electrode) can be used for digital camera applications with high pixel density.
[0178] The method for preparing the above-mentioned infrared organic detector array comprises the following general steps:
[0179] (1) Base cleaning;
[0180] (2) forming a first electrode film and performing ultraviolet irradiation or oxygen plasma cleaning;
[0181] (3) Preparation of the first electrode interface layer film;
[0182] (4) P-type semiconductor material and N-type semiconductor material are mixed in a certain mass ratio to prepare a photosensitive layer
[0183] (5) Preparation of the second electrode interface layer film;
[0184] (6) Preparation of the second electrode;
[0185] (7) Preparation of encapsulation layer.
[0186] The photosensitive layer is prepared by a method selected from solution film formation or vacuum thermal evaporation deposition.
[0187] The preparation of the charge transport layer is independently selected from one or more of solution film formation, sol-gel film formation, vacuum thermal evaporation, atomic layer deposition, chemical vapor deposition, electrodeposition, and anodization.
[0188] The preparation of the first electrode and the second electrode are independently selected from one or more of vacuum thermal evaporation, electron beam evaporation, molecular beam evaporation or plasma sputtering, atomic layer deposition or liquid film formation followed by reduction conversion, electroplating or electrodeposition.
[0189] The encapsulation layer is prepared by vacuum thermal evaporation, chemical vapor deposition, atomic layer deposition, plasma sputtering, and liquid film formation.
[0190] The encapsulation layer can protect the infrared organic detector from moisture or oxygen. The encapsulation layer may include: an inorganic film including silicon nitride (SiNx), silicon oxide (SiOx), indium tin oxide, indium zinc oxide or any combination thereof; an organic film including polyethylene terephthalate, polyethylene naphthalate, polycarbonate, polyimide, polyethylene sulfonate, polyoxymethylene, polyarylate, hexamethyldisiloxane, acrylic resin (e.g., polymethyl methacrylate, polyacrylic acid, etc.), epoxy resin (e.g., aliphatic glycidyl ether (AGE: aliphatic glycidylether), etc.) or any combination thereof, or a combination of an inorganic film and an organic film.
[0191] Embodiment 11
[0192] This embodiment also provides an infrared organic detector chip, which includes the infrared organic detector array described in Embodiment 10.
[0193] This embodiment can use the infrared organic detector chip of the present invention to detect the object to be detected, such as Fig.14 As shown. When the detection device uses a visible light detector chip as a photosensitive chip, if the light source emits visible light, the visible light cannot pass through the silicon wafer due to the obstruction of the silicon wafer. At this time, the visible light detector chip cannot detect the object to be tested. However, when the detection device uses the infrared organic detector chip described in the present invention as a photosensitive chip, even if there is obstruction by the silicon wafer, the infrared light emitted by the light source acts on the object to be tested and is reflected by the object to be tested. The infrared light passes through the silicon wafer and is detected by the infrared organic detector chip of the present invention. Therefore, the detection device equipped with the infrared organic detector chip of the present invention can clearly detect the object to be tested. The detection device includes but is not limited to industrial cameras, medical equipment, etc.
[0194] like Fig.15 , a schematic diagram of the present embodiment using a visible light detector for detection imaging, through Fig.15 It can be seen that the text on the back of the silicon wafer cannot be detected. Fig.16 This is a schematic diagram of the present embodiment using the infrared organic detector described in Embodiment 8 to perform detection imaging. Fig.16 It can be seen that the text on the back of the silicon wafer can be detected.
[0195] The infrared organic detector chip described in this embodiment can be applied in the following aspects:
[0196] 1. It can be an industrial camera used to detect and identify defects, foreign matter, cracks and other problems on the surface of materials.
[0197] 2. It can also be used in medical diagnosis. Infrared light can penetrate the skin and other biological tissues, providing deeper details and resolution.
[0198] 3. It can also be used in food safety, specifically to detect contaminants, ingredients and quality in food.
[0199] 4. It can also be used in environmental monitoring to help monitor environmental parameters such as atmospheric pollutants, water quality and soil moisture content.
[0200] Obviously, the above embodiments of the present invention are only examples for clearly explaining the present invention, and are not intended to limit the implementation methods of the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention shall be included in the protection scope of the claims of the present invention.
Claims
1. An infrared organic detector, Features: The infrared organic detector comprises a first electrode, a second electrode, a photosensitive layer arranged between the first electrode and the second electrode, and a charge transport layer arranged between the first electrode and the photosensitive layer and / or between the second electrode and the photosensitive layer; Wherein, the photosensitive layer comprises an infrared absorbing compound, and the absorption edge of the infrared absorbing compound is between 900nm and 2000nm.
2. An infrared organic detector according to claim 1, Features: When the first electrode is a cathode, the charge transport layer between the first electrode and the photosensitive layer is an electron transport layer, and the electron transport layer includes an N-type material; The corresponding second electrode is an anode, and the charge transport layer between the second electrode and the photosensitive layer is a hole transport layer, which includes a P-type material.
3. The infrared organic detector according to claim 1, Features: When the first electrode is an anode, the charge transport layer between the first electrode and the photosensitive layer is a hole transport layer, and the hole transport layer includes a P-type material; The corresponding second electrode is a cathode, and the charge transport layer between the second electrode and the photosensitive layer is an electron transport layer, which includes an N-type material.
4. The infrared organic detector according to claim 1, Features: The charge transport layer includes two or more transport sublayers.
5. An infrared organic detector according to claim 4, Features: When the charge transport layer is an electron transport layer, the LUMO energy level difference between two adjacent transport sublayers is less than or equal to 1.0 eV.
6. The infrared organic detector according to claim 4, Features: When the charge transport layer is a hole transport layer, the HOMO energy level difference between two adjacent transport sublayers is less than or equal to 1.0 eV.
7. The infrared organic detector according to claim 1, Features: The infrared absorbing compound includes an N-type receptor material of the following structural formula: In formula (I), n represents the number of repeating units of the polymer. When n is 1, the copolymerization unit in formula (I) does not exist; when n is a natural number between 2 and 10,000, the copolymerization unit in formula (I) exists; A is an electron withdrawing group; B is a π bridge; C and the copolymerization unit are both conjugated aromatic ring units.
8. An infrared organic detector according to claim 7, Features: The A unit is selected from any one of the following structures: The dotted line ① represents the connection site between the copolymer unit and the A unit, and the dotted line ② represents the connection site between the B unit and the A unit; X 1 Each is independently selected from hydrogen, halogen, trifluoromethyl, cyano, nitro, C1-C30 straight chain, branched or cyclic alkyl, C1-C30 straight chain, branched or cyclic alkoxy, C1-C30 straight chain, branched or cyclic alkylthio; Any one or more hydrogen atoms in the A unit are not substituted by other atoms and / or groups, or are independently substituted by protium, deuterium or tritium atoms.
9. The infrared organic detector according to claim 7, Features: The B units are each independently selected from the formula The group shown, or The group shown, or The group shown, or The groups shown, or not present; Among them, R 1 One or more independently selected from hydrogen, halogen, ester, hydroxyl, nitro, cyano, alkyl, alkyl derivative, alkylene, alkylene derivative, aralkyl, aralkyl derivative; One or more carbon atoms on the alkyl derivative, alkylene derivative or aralkyl derivative are substituted by one or more of oxygen atoms, amino groups, sulfone groups, carbonyl groups, aryl groups, olefin groups, alkynyl groups, ester groups, cyano groups and nitro groups; and / or One or more hydrogen groups on the alkyl derivative, alkylene derivative or aralkyl derivative are replaced by one or more of halogen, hydroxyl, amino, carboxyl, cyano, nitro, aryl, alkene or alkyne groups; Y 1 Independently selected from O, S, Se or NR 1 ; Any one or more hydrogen atoms in the B unit are not substituted by other atoms and / or groups, or are independently substituted by protium, deuterium or tritium atoms.
10. The infrared organic detector according to claim 7, Features: The C unit is selected from any one of the following structures: Among them, R 2 is independently selected from one or more of a hydrogen atom, a halogen, an ester group, a hydroxyl group, a nitro group, a cyano group, an alkyl group, an alkyl derivative, an alkylene group, an alkylene derivative, an aralkyl group, an aralkyl derivative; or is absent; One or more carbon atoms on the alkyl derivative, alkylene derivative or aralkyl derivative are substituted by one or more of oxygen atoms, amino groups, sulfone groups, carbonyl groups, aryl groups, olefin groups, alkynyl groups, ester groups, cyano groups and nitro groups; and / or One or more hydrogen groups on the alkyl derivative, alkylene derivative or aralkyl derivative are replaced by one or more of halogen, hydroxyl, amino, carboxyl, cyano, nitro, aryl, alkene or alkyne groups; Y 2 Independently selected from O, S, Se or NR 1 ; Z 1 Each independently selected from N, C, Si or Ge; Any one or more hydrogen atoms in the C unit are not substituted by other atoms and / or groups, or are independently substituted by protium, deuterium or tritium atoms.
11. The infrared organic detector according to claim 7, Features: The copolymerization unit is selected from any one of the following structural formulas and combinations thereof: Among them, R 3 Each independently selected from hydrogen, halogen, trifluoromethyl, cyano, nitro, C1-C60 straight chain, branched or cyclic alkyl, C1-C60 straight chain, branched or cyclic alkoxy, C1-C60 straight chain, branched or cyclic alkylthio, alkyl substituted aryl; the alkyl in the alkyl substituted aryl is a straight chain or branched alkyl with 1 to 60 carbon atoms, and the aryl is a benzene ring or a thiophene ring; Y 3 Independently selected from O, S, Se or NR 1 ; Z 2 Each independently selected from N, C, Si or Ge; Any one or more hydrogen atoms in the copolymerized units are not substituted by other atoms and / or groups, or are independently substituted by protium, deuterium or tritium atoms.
12. An infrared organic detector array, Features: The infrared organic detector array includes a plurality of picture elements, and the picture elements include the infrared organic detector as claimed in claim 1.
13. The infrared organic detector array according to claim 12, Features: The infrared organic detector array also includes a substrate; the substrate is a pixel readout circuit composed of silicon-based complementary metal oxide semiconductor transistors or thin film transistors.
14. An infrared organic detector chip, Features: Comprising the infrared organic detector array as claimed in claim 12.