Electrode for energy storage device

The formation of composite particles through an electrostatic deposition process solves the handling and safety issues caused by the use of solvents in traditional battery manufacturing, achieves uniformity of high-performance electrodes and the manufacture of efficient electrochemical energy storage devices, and reduces manufacturing costs and energy consumption.

CN118872083APending Publication Date: 2024-10-29AM BATTERIES INC
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202380019595.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-05
Filing Date
2023-01-31
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Traditional battery manufacturing methods use solvent-based methods, which lead to handling, ventilation and safety issues, and require drying time to allow liquid solvents to evaporate or fuse, affecting the uniformity of electrode coatings and the performance of electrochemical energy storage devices.

Method used

The electrostatic deposition process is used to form composite particles, including adhered binder particles and conductive particles, which are uniformly deposited on the conductive current collector through air flow aeration and fluidization to form a high-performance electrode, avoiding the use of solvents.

Benefits of technology

The uniformity of the solvent-free electrode coating and the formation of high-performance electrodes are achieved, the energy consumption and manufacturing costs during the manufacturing process are reduced, and the energy density, power density and cycle life of the battery are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118872083A_ABST
    Figure CN118872083A_ABST
Patent Text Reader

Abstract

An electrode for an electrochemical energy storage device formed by an electrostatic deposition process, the electrode employing composite particles comprising active material (AM) particles with an adhesive binder and optionally conductive particles, the individual constituent particles forming a sufficient interaction force to form an effective composite particle, it can overcome electrostatic charge, fluidization, and / or particle separation during mechanical transport. The secondary binder particles are depolymerized to form sub-particles that adhere to AM particles having a predetermined morphology. The smaller conductive particles, typically carbon black (CB) or similar carbon, are bonded to the binder and adhered to the AM particles. The result is that the composite particles are adhered to withstand separation forces caused by application of electrostatic deposition onto the current collector. Applying a plurality of composite particles in a uniform pattern and a determined load to a conductive current collector promotes stable energy density, power density, and cycle life of the electrochemical energy storage device.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to U.S. Provisional Application No. 63 / 304,907, filed on January 31, 2022, entitled “Electrode for Energy Storage Device,” and assigned Serial No. 17 / 713,722, filed on April 5, 2022, entitled “Electrode for Energy Storage Device,” and assigned Serial No. 17 / 713,722. The entire contents of the foregoing provisional and non-provisional applications are incorporated herein by reference. Background Art 1. Technical Field

[0004] The present disclosure relates to electrochemical energy devices and related manufacturing methods. The disclosed electrochemical energy devices generally include an electrode, wherein the electrode includes a coating formed at least in part by depositing dry composite particles onto a conductive substrate by an electrostatic deposition process. The composite particles include active material particles and binder particles surrounding the active material particles, the binder particles are generally formed by deagglomeration of binder agglomerates, and adhere to the surface of the active material particles by inter-particle adhesion forces. 2. Background technology

[0006] Electrochemical energy storage devices have electrodes comprising a coating connected to a conductive current collector layer (usually a copper or aluminum sheet). The coating can include cathode active materials and anode active materials, and is typically combined with conductive materials and binder materials to form a structure that easily discharges and accepts charge (recharges) depending on the applied electrical load or charging potential. The formation of electrochemically active materials, binders, and conductive particles can vary depending on the applicable battery chemistry and production methods.

[0007] Conventional battery manufacturing methods use solvent-based methods to form electrodes. This typically involves a binder solution or suspension used to flow or apply electrochemically active materials and conductive particles to a conductive current collector foil. Conventional methods typically involve solvents, which pose handling, ventilation, safety issues, and require drying time to allow the liquid solvent to evaporate or fuse the ingredients in the coating.

[0008] It is generally desirable to form a coating having a uniform dispersion of electrochemically active materials, conductive particles, and a binder at a density that promotes electrical connectivity between the electrochemically active materials and the current collector to produce a battery having optimal energy density, power density, and cycle life. It is desirable to improve the method of applying the coating and the electrochemically active materials formed thereby. The methods and apparatus of the present disclosure meet these and other objectives. Summary of the invention

[0009] An electrode for an electrochemical energy storage device formed by an electrostatic deposition process is provided, wherein the electrode uses composite particles, wherein the composite particles include electrochemically active material (or active material, "AM)" particles with adhered binder particles and optional conductive particles, and sufficient interaction is formed between the individual component particles to form effective composite particles, which can overcome / resist the particle separation forces during electrostatic charging and fluidization during the electrostatic deposition process.

[0010] Commercially available adhesive materials or conductive materials are usually present in the form of agglomerates, often referred to as secondary particles, which are formed by physical interactions of multiple primary particles. According to the present disclosure, adhesive agglomerates are depolymerized to form sub-particles, and the sub-particles are adhered to AM particles with predetermined and / or desired morphologies. It is worth noting that conductive agglomerates are also depolymerized to form sub-particles. Sub-particles include one or more primary particles that are smaller in size than the original agglomerates. When forming the advantageous energy storage device of the present disclosure, adhesive particles and conductive particles are introduced in the form of sub-particles.

[0011] Typically, according to the present disclosure, carbon black (CB) or similar carbon is bonded to a binder and, together with the binder, adheres to the AM particles. The result is that the composite particles exhibit sufficient adhesion to withstand the separation forces applied during electrostatic deposition. In a typical electrostatic spray deposition (ESD) process, the composite particles disclosed herein are aerated and fluidized by a gas stream and are carried by the gas stream to be deposited on a conductive current collector in a uniform pattern and density. Alternative electrostatic deposition methods may also be used.

[0012] The composite particle layer deposited on the current collector can be further densified according to the present disclosure to form an electrode of a battery. The uniformity of the deposited composite particle layer is critical to the performance of the resulting battery. The uniformity of the deposited composite particle layer requires, in particular, stoichiometric consistency between the deposited layer and the raw material powder mixture, as well as stoichiometric consistency and geometric consistency within the deposited layer.

[0013] In the battery industry, there is great commercial interest in applying electrostatic deposition techniques to form solvent-free electrode coatings for lithium-ion batteries. Solvent-free electrode coating techniques are attractive because, among other things, ESD techniques can significantly reduce energy consumption in the manufacturing process and significantly reduce the manufacturing costs of the battery. In principle, the use of electrostatic deposition techniques allows for simpler and more flexible electrode coatings in the manufacture of energy storage devices, since the composite electrode powder is deposited directly on the metal current collector by an electrostatic spray deposition process.

[0014] In conventional applications, electrostatic deposition techniques are widely used for dry powder coating of conductive parts. In conventional applications of electrostatic deposition coating techniques, coating quality, especially coating uniformity, is directly related to and dependent on the properties of the particles contained in the coating powder. These properties include particle size, relative dielectric constant, conductivity, density, morphology, etc. According to the present disclosure, the properties of the particles associated with the coating powder are selected such that the electrostatically deposited coating formed with the disclosed composite particles advantageously promotes / provides a uniform electrode for battery applications.

[0015] The configurations herein are advantageously able to meet the demand for reliable batteries in a range of end-use applications, particularly including electric vehicles (EVs), which use considerable current draw to provide adequate vehicle performance. Unfortunately, as described above, conventional battery manufacturing methods employ a solvent-based approach to form electrodes. This typically involves a binder solution or suspension for flowing or applying electrochemically active materials and conductive particles to a conductive current collector foil. Conventional processes involve solvents, which present handling, ventilation, safety issues, and require drying time to allow the liquid solvent to evaporate or fuse the components in the coating. Therefore, the configurations herein provide electrodes comprising composite particles by applying a dry powder to a conductive current collector using an electrostatic deposition method, substantially overcoming the above-mentioned disadvantages of solvent-based battery formulations.

[0016] As disclosed herein, the desired morphology or structure of the composite particles is obtained by deagglomeration, mixing and adhesion between the constituent particles to form active material (AM) particles with an adhesive binder and optional conductive particles in a form that can withstand an electrostatic deposition process. After deposition onto a conductive current collector substrate, the disclosed AM particles form / define the precise loading and microstructure of a high-performance battery. It is worth noting that "loading" refers to the unit coating mass on a specific area, usually expressed in mg / cm 2 count.

[0017] As disclosed herein, a favorable electrode is formed by electrostatically depositing composite particles on a conductive current collector to form a high-efficiency electrode / electrochemical energy storage device. The disclosed electrode / electrochemical energy storage device generally includes a plurality of composite particles suitable for electrostatic deposition onto a conductive current collector substrate, wherein each composite particle includes one or more active material particles, binder particles surrounding the active material particles, and conductive particles adhered to the binder particles. The disclosed binder particles are generally formed by depolymerizing binder agglomerates to form sub-particles. The binder particles adhere to the surface of the active material particles through interaction forces sufficient to withstand the powder mixing process. The interaction is also sufficient to overcome the separation force caused by the electrostatic deposition process, which is ideal for maintaining the structure of the composite particles when the composite particles are formed on the conductive current collector substrate by the electrostatic deposition process.

[0018] The disclosed electrochemical energy storage devices and methods of producing the same are highly advantageous in providing effective energy storage functionality without requiring solvent-based manufacturing processes.

[0019] Additional features, functions, and benefits of the disclosed electrochemical energy storage devices and related methods of manufacture will become apparent from the following detailed description, particularly when read in conjunction with the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] The foregoing and other features will become apparent from the following description of specific embodiments disclosed herein, as shown in the accompanying drawings, in which like reference numerals refer to the same parts in different views. The drawings are not necessarily drawn to scale, emphasis instead being placed upon illustrating the principles of the invention.

[0021] Figure 1 is a schematic diagram of a composite particle, wherein composite particle 101C reflects a composite particle disclosed herein;

[0022] Figure 2 The configuration of the electrochemical energy storage device is shown Figure 1 Background / Exemplary Systems of Composite Particles (Composite Particles 101C);

[0023] Figure 3A and 3B Shows Figure 1 Example compositions of composite particles;

[0024] Figure 4 Shows Figure 1-3B The formation process of composite particles in

[0025] Figures 5A-5C SEM images of mixed powders of sample 1, sample 3 and sample 4 respectively;

[0026] Figures 6A-6C SEM images of larger areas of mixed powders of sample 1, sample 3, and sample 4, respectively;

[0027] Figures 7A-7C EDS images (nickel mapping) of mixed powders of sample 1, sample 3, and sample 4, respectively;

[0028] Figures 8A-8C EDS images (fluorine mapping) of mixed powders of sample 1, sample 3, and sample 4, respectively;

[0029] Fig. 9 is a graph showing the bonding strength of electrodes prepared by electrostatic spray deposition of powders using different mixing times and speeds according to the present disclosure;

[0030] Fig.10is a SEM image of composite particles (NCM 622 / PVDF / carbon) deposited on an Al substrate according to the present disclosure;

[0031] Fig.11 is an EDS mapping image of composite particles (NCM 622 / PVDF / carbon) deposited on an Al substrate according to the present disclosure, showing the distribution of Ni active particles;

[0032] Fig.12 is an EDS mapping image of composite particles (NCM 622 / PVDF / carbon) deposited on an Al substrate according to the present disclosure, showing the distribution of carbon particles relative to Ni active particles;

[0033] Fig.13 is an EDS mapping image of composite particles (NCM 622 / PVDF / carbon) deposited on an Al substrate according to the present disclosure, showing the distribution of PVDF binder particles relative to Ni active particles;

[0034] Fig.14 is a graph of resistance versus mixing time of an electrode fabricated by depositing composite particles on a substrate using ESD; and

[0035] Fig.15 is a graph of bonding strength versus mixing time for electrodes fabricated by depositing composite particles on a substrate using ESD. DETAILED DESCRIPTION

[0036] Described below are exemplary methods and devices for forming and configuring composite particles in electrochemical energy storage devices such as rechargeable batteries. Other particle deposition methods may be used to bond composite particles to current collectors or other energy storage devices to store and release electrical energy (electrons) to provide electrical current in a controlled and efficient manner.

[0037] As used herein, the term "particle" generally refers to a granular quantity of a particulate material suitable for mixing and interacting with other particles. The particle morphology may be spherical or any other form. Examples involving single particles are intended to illustrate the occurrence or interaction of some or all of the particles (including powder and granular forms) that affect the particle quantity. It should also be noted that in battery terminology, "active charge material" is generally referred to as "electrochemically active material" or "electrode active material". Depending on the context, the electrostatically deposited material so deposited disclosed herein may be referred to as a "coating".

[0038] Particle agglomeration usually occurs in loose granular materials, including electrochemically active materials, binder materials and conductive materials related to the manufacture of electrochemical energy storage devices according to the present disclosure. All of these materials exist in the form of particles and may also exist in the form of agglomerates, which means that multiple primary particles interact with each other through relatively weak forces and are broken by stirring and mixing. Common nomenclature represents agglomerates as secondary particles, and once stirred, they are broken into primary particles or sub-particles. Although the processes and methods discussed herein are generally used to form discrete primary particles from sub-particles of agglomerates that are broken, stirred or stirred, the particles defined herein include primary particles, secondary particles, sub-particles of agglomerates, and any interaction or combination between specific types of particles. In other words, although primary particle clusters, which are generally referred to as secondary particles or agglomerates, are generally expected to be broken into smaller particles when stirred, some agglomerates may remain and still define particles of corresponding active materials, binders or conductive materials, i.e., particles and / or sub-particles of any form thereof. Therefore, a particle can be broken into multiple sub-particles, but each sub-particle is still a particle. Furthermore, the force applied during agitation may be sufficient to break up agglomerated particles.

[0039] Figure 1 is a schematic diagram of the composite particles disclosed herein. The configuration herein applies solvent-free (dry) electrostatic spray deposition (ESD) coating technology to the manufacture of battery composite electrodes with high uniformity. The present disclosure also enables a composite powder mixing process to produce a suitable composite powder mixture for ESD electrode coating. Alternative applications include any electrochemical storage device, such as a fuel cell.

[0040] The battery has a cathode and an anode. In a typical lithium-ion battery, the cathode and anode are based on a composite electrode powder mixture. The composite electrode powder mixture generally contains active electrode material particles (AM), binder material particles (Binder) and conductive material particles (CB). The active electrode materials include cathode materials such as lithium metal oxide-based cathode materials: NCM (lithium nickel cobalt manganese oxide), LMO (lithium manganese oxide), NCA (lithium nickel cobalt aluminum oxide), LCO (lithium cobalt oxide) and lithium polyanion-based positive electrode materials: LFP (lithium iron phosphate), LiMn x Fe 1-x PO4, Li2FeSiO4 and carbon-based anode materials, graphite, Si, silicon-based composite materials, SiO x , lithium alloy materials or lithium transition metal oxide anode materials. In a typical sodium ion battery, the cathode material includes a sodium transition metal oxide, such as Na 2 / 3 Fe 1 / 2 Mn 1 / 2O2, sodium polyanion materials such as Na2MnSiO4, Prussian blue analog cathode materials such as Na2MnFe(CN)6. Anode materials include carbonaceous anodes, sodium alloy materials, sodium transition metal oxides or Prussian blue analog anode materials. Transition metal oxide-based cathode materials (such as NCM) are semiconductors with 10 -6 Up to 10 -7 Electronic conductivity in S / cm.

[0041] Typical binder materials are polymer materials, such as PVDF (polyvinylidene fluoride), PTFE (polytetrafluoroethylene), PEO (polyethylene oxide) or PMMA (polymethyl methacrylate), SBR (polystyrene butadiene rubber binder), CMC (carboxymethyl cellulose binder) or PAA (polyacrylic acid), which are electrical insulators. The binder material can also be a polymer electrolyte, such as PEO / lithium trifluoromethanesulfonate polymer electrolyte. In addition, the binder can be a solid electrolyte composite material composed of an inorganic solid electrolyte and a polymer binder, a polymer electrolyte binder or an organic binder, such as a Li3InCl6 / PMMA composite material, a LLZO / polymer electrolyte composite material.

[0042] The conductive material may include conductive carbon black (CB), carbon nanotubes or graphene. In addition, the composite electrode may contain some functional additives. These additives may be, for example, silicon dioxide, aluminum oxide, zirconium oxide or any combination thereof.

[0043] The true density of the cathode material is typically 4-5 g / cc for NCM and 3.6 g / cc for LFP. The true density of the binder is typically in the range of 1-2 g / cc. The typical particle size of the active material is in the range of 1-40 μm. The binder material typically has a primary particle size of 100-1000 nm and an agglomerate size of 5-30 nm. The conductive material typically has a primary particle size of 40-80 nm. The conductive current collector is typically Al foil and Cu foil, with or without a primer layer that enhances the adhesion between the coating and the conductive substrate. Such an adhesion layer can be applied to the conductive substrate before deposition.

[0044] refer to Figure 1, an electrode formed by electrostatic spray deposition (ESD) for an electrochemical energy storage device according to the present disclosure includes a plurality of composite particles suitable for electrostatic deposition onto a conductive current collector substrate. Each composite particle (or at least the vast majority of the composite particles) of the plurality of composite particles includes active material particles and binder particles surrounding the active material particles. According to the present disclosure, the binder particles are formed by decomposing the binder agglomerates into sub-particles or directly introducing prefabricated sub-particles. In either case, the binder particles adhere to the surface of the active material particles by a binding force that is greater than the interaction force generated during the agitation of the binder agglomerates based on the force introduced into the system by such agitation. Conductive additives may be added to form a composite material.

[0045] exist Figure 1 In the figure, particle range 100 depicts an exemplary cathode material for an electrochemical energy storage device. In the composite electrode powder mixture, the weight ratio of active material is generally higher than 80%, and the weight ratio of binder and conductive material is lower than 20% to enable the battery to have sufficient weight energy density and acceptable / beneficial power density. The composite electrode powder mixture is prepared by a mixing process to uniformly disperse the component particles. Figure 1 Several dispersion patterns of particles 101A, 101B, and 101C of the constituent particles in a composite electrode powder mixture that is thoroughly mixed by dry blending are shown. The constituent particles include AM, binder, and conductive particles; however, in some configurations, conductive materials are not required and / or included in the composite electrode, as will become apparent in the following discussion.

[0046] Typically, AM particles 111 are the largest particles, binder particles 112 are smaller particles, but there are variations (shown as hatched lines), and conductive particles 113 (shown as solid lines) have the smallest particle size range. However, in specific embodiments, the sizes and size relationships may vary greatly. In particle 101A, binder 112 either has a large sub-particle size or is in the form of agglomerates. The active material 111 particles retain their original morphology during dry mixing. In static powder form, all particles are well dispersed, but there is no strong interaction between AM 111, binder 112 and CB (conductive) particles 113.

[0047] Particle 101B shows that the binder 112 agglomerates are favorably broken up during the mixing process, and the sub-particle size is smaller than that of the active material 111. The active material particles retain their original morphology during the dry mixing process. Like 101A, in static powder form, particles 111, 112, and 113 can be well dispersed, but there is no strong interaction force between the AM, binder, and CB particles.

[0048] Particle 101C depicts a composite particle in which the binder agglomerates are broken up during the mixing process and the sub-particles 112 are smaller in size than the active material 111. The active material particles retain their original shape during the mixing process. In static powder form, the binder particles and the conductive particles are discretely coated on the surface of the active material particles by surface fusion, van der Waals attraction, or various potential physical interactions and chemical bonds. The composite particle 101C is suitable for electrostatic deposition of the binder-based sub-particles onto a current collector substrate, agitated to break up the agglomerates, and the interaction force is sufficient to withstand the separation forces caused by material processing, electrostatic deposition, and post-deposition processing on the substrate to maintain the morphology of the composite particle 101C.

[0049] It is noteworthy that the significant effect on the binder / active material particle ratio resulting from the deagglomeration of the binder particles by the mixing process of the present disclosure can be calculated on a theoretical basis. Thus, as shown in Table 1 below, an average particle size of 0.1 μm binder particles increases the binder / active material particle ratio to 53819, compared to 431 for 0.5 μm binder particles and 54 for 1 μm binder particles. Thus, according to the present disclosure, the distribution of binder particles relative to active particles (assuming 10 μm) is increased by several orders of magnitude.

[0050] Table 1

[0051]

[0052] A variety of AM particle and composite particle formulations can be achieved. It should be noted that the difference between the component particles and the formed composite particles, the component particles are AM, binder and conductive material, which are usually obtained as a uniform loose particle material, while the formed composite particles are formed by electrostatic deposition by particle-particle interaction forces. In an exemplary arrangement, the active material is formed by a transition metal oxide and is used as a cathode material for an electrochemical energy storage device. Typical cathode materials include NCM (lithium nickel cobalt manganese oxide), LFP (lithium iron phosphate), LCO (lithium cobalt oxide) or other suitable chemical formulations, usually based on the form that can accept and release lithium ions. Prior to deposition, the cathode material is usually formulated using a proprietary process (rather than a bulk commodity). The active material formed by the disclosed method can also be an anode material for an electrochemical energy storage device. Exemplary configurations of active materials are used for rechargeable batteries with chemistries defined by rechargeable lithium batteries, lithium ion batteries, rechargeable Li-S batteries, solid-state batteries, rechargeable sodium batteries and sodium ion batteries. The binder particles are usually formed by one or more of polymer materials, polymer electrolytes and solid electrolyte composites; several specific compounds are listed above.

[0053] Figure 2 shows the configuration for the battery Figure 1Background / Exemplary System of Composite Particles. The ESD manufacturing process 200 includes an electrostatic deposition applicator 215 and a hopper 216. The raw material 214 includes a loose amount of composite particles 101C as described above. The composite particles 101C are produced by a mixer 130 having an agitator 132 or a similar method for mixing, combining and adhering the composite particles 101C. The source of loose particles includes active material 150-1, adhesive particles 150-2, and optional conductive particles 150-3 (collectively referred to as 150). The source 150 is fed into the mixer 130 in a predetermined amount, typically at least 80% by weight of the active material. The source 150 comes from any suitable commercial or industrial supply, is typically a homogeneous loose raw material, and has the texture of granules, particulates or powder. In the discussion herein, granules and powders should be considered interchangeable.

[0054] After agitation, the binder particles are typically between 200-1000 nm and the conductive particles are between 100-500 nm. After agitation, the mixer 130 contains the composite electrode mixture 160 for the raw material 214. The AM particles are typically in the range of 1-40-4 and are much larger than the adherent binder and conductive particles, which will be discussed further below.

[0055] In such Figure 2 In the electrostatic deposition device 250 shown, Figure 1 The composite particles of C are depicted as constituent particles of the cathode material. The active material may be a cathode material or an anode material, formed from respective cathode material or anode material particles. The composite particles from the feedstock 214 are aerated and fluidized by a pressurized gas stream (usually dry air). The fluidized composite particles carried by the gas stream are charged by an electrostatic applicator 215, travel in an electric field, and are ultimately deposited on a grounded conductive current collector 254 to form a composite particle layer 252. The composite particles fluidized and carried by the gas stream are charged in the electrostatic applicator 215 by corona charging or friction charging.

[0056] The product output by the electrostatic deposition manufacturing process 200 is a coating sheet 253, including a composite particle layer 252 and a substrate 254. The electrostatic deposition applicator 215 can be any suitable electrostatic deposition device. A spraying process is usually involved, but other electrostatic deposition methods can also be used. The coating sheet 253 is densified to form an electrode for an electrochemical energy storage device. The coating sheet 253 can be preheated before densification. The densification process can be carried out with or without heating. A cathode or anode can be manufactured by the above method. The densification process can be repeated, for example, multiple times. For electrostatic charging of the composite particles, the electrostatic applicator can use any suitable electrostatic method. Electrostatic applications include corona charging, friction charging, direct electrode induction charging or other suitable charging methods.

[0057] Electrochemical energy storage devices (e.g., lithium-ion batteries) have a cathode, an anode, a separator, and an electrolyte. The cathode typically includes an active material such as NCM, a binder material such as PVDF, and a conductive material such as carbon black. The anode typically includes an active material such as graphite, a binder material such as PVDF or SBR / CMC binder, and / or a conductive material such as carbon black. The separator is typically a porous polymer film that separates the cathode and the anode and allows ion transport between the cathode and the anode. The electrolyte is typically a lithium salt solution, such as a solution of a LiPF6 salt and an EC / DMC / EMC solvent, which provides ion conduction between the cathode and the anode.

[0058] In load mode or discharge mode, oxidation occurs at the anode and reduction occurs at the cathode. During charging, reduction occurs at the anode and oxidation occurs at the cathode. The energy stored in an electrochemical energy storage device depends on the electrochemical energy stored in the active material and also on the amount of active material in the electrode. In addition, the uniformity of current distribution in an electrochemical energy storage device significantly affects the cycle life of the device. The uniformity of current distribution is directly related to the uniformity of the electrode. The structural properties of the electrode (such as porosity and thickness) affect the power capacity of the electrochemical energy storage device.

[0059] The properties affected by the formation and stratification of charged materials include electrode uniformity, active material loading in the electrode, electrode porosity, electrical conductivity, electrode processability, which are directly related to the energy density, power density, and cycle life of the resulting battery.

[0060] In the electrostatic process 200, the charge of a particle is related to its relative dielectric constant and size by the following equation:

[0061]

[0062] in:

[0063] r = particle radius,

[0064] E = electric field strength,

[0065] e = electron charge,

[0066] k = electron mobility,

[0067] n = electron concentration,

[0068] t = time,

[0069] ε0 = absolute dielectric constant, and

[0070] ε r = Relative dielectric constant of powder

[0071] Typical particle sizes for cathode materials range from 1-40 μm. Typical primary particle sizes for PVDF binders are 200-300 nm. Typical primary particle sizes for conductive carbon are 40-50 nm. According to the above equation, the charges of the individual powder components during electrostatic deposition will vary by several orders of magnitude, since the maximum charge of the particle is directly related to the square of the particle radius.

[0072] The cathode material generally has a much higher relative dielectric constant than the polymer binder material. For example, the relative dielectric constant of PVDF at 21°C is about 8-10, and the relative dielectric constant of lithium nickel oxide-based cathode materials is on the order of 1000.

[0073] The relaxation time t for the charge dissipation of an ideal charged body is given by:

[0074] τ=ε o ε r / σ

[0075] in:

[0076] ε r = relative dielectric constant of the powder, and

[0077] σ = electronic conductivity of the powder

[0078] The electronic conductivity of NCM cathode materials is typically 10 -6 -10 -7 S / cm, PVDF<10 -14 S / cm, which results in several orders of magnitude difference in the relaxation time for charge dissipation.

[0079] Based on the above analysis, the active material particles, binder particles and conductive material particles have different electrostatic deposition behaviors during the electrostatic deposition process due to the significant differences in chargeability and charge dissipation time caused by differences in conductivity, dielectric constant, particle size and density.

[0080] Furthermore, differences in particle size, particle density, morphology, surface roughness and, therefore, surface energy will exhibit different behaviors as they relate to aerodynamic effects during powder fluidization and mechanical transport to the coating substrate.

[0081] If there are no strong interaction forces between the particles in the mixture, significant separation may occur during the coating process due to differences in the behavior of electrostatic deposition and fluidization related to the powder properties, which translates into a detrimental effect on the coating uniformity in terms of composition, microstructure and size. For example, conventional methods result in deposited layer 252 having a different stoichiometry than raw material 214 due to different deposition patterns of the individual component particles.

[0082] In the electrostatic deposition process 200 using conventional technology, when the powder particles pass through the spatial charging zone in the corona charging, friction charging or direct flat electrode electrostatic charging system, the active material particles, binder particles and conductive material particles (such as those formed in 101A and 101B) are charged separately. Due to the difference in charging rate and charge dissipation time, each charged particle is deposited on the current collector, resulting in unevenness in the deposited layer.

[0083] In the formation process of the composite particles 101C according to the present disclosure, small binder particles and conductive material particles are attached / adhered to the surface of the active material particles to form composite particles. During the aeration or mechanical transport and deposition of the composite particles composed of active material particles with binder and conductive material particles attached to the surface, the composite particles are charged and deposited, which results in uniform deposition on the current collector substrate 254. In addition, due to the high resistivity of the binder particles 112, the charge dissipation time of the composite particles is longer than that of the pure active material particles, which enables electrostatic forces to play a role during the post-coating process until the curing operation of the binder can be performed. Therefore, the composition of the composite particles 101C in the raw material 214 electrode powder mixture is particularly conducive to electrostatic deposition to achieve a high degree of uniformity.

[0084] Figure 3A and 3B Shows Figure 1 Example composition of composite particles. Figure 1-3A -3B, Figure 3A Composite particle 101C is shown having AM particles 111 and adhered binder particles 112 . Figure 3B It is shown that the composite particle 101C also includes conductive particles 113. According to the arrangement of the mixer 130, the composite particle 101C can be formed by mixing the conductive particles 113, the active material particles 111, and the binder particles 112 at the same time. In an alternative configuration, the composite particle 101C also includes bonding the conductive particles 113 to adhere to the surface of the binder particles 112, and then the composite particle 101C is formed by bonding the bonded binder and conductive particles to the surface of the AM particles 111.

[0085] In order to obtain a composite electrode powder mixture formed by composite particles 101C, any mixing / particle coating equipment, such as an impact mixer or a shear mixer, can be used. The binder agglomerates are broken into sub-particles, and the conductive material agglomerates are broken into smaller particles. These sub-particles are attached / adhered to the surface of the active material particles by surface fusion, van der Waals attraction, or various potential physical interactions or chemical bonds to generate sufficiently large interaction forces between individual particles to form effective composite particles that can overcome electrostatic charging, fluidization, mechanical transport and / or particle separation during deposition.

[0086] Figure 4 Shows Figure 1-3B The process of forming composite particles (e.g., composite particles 101C) in the electrostatic deposition system 200 is described in detail. An important feature of mixing and agitation is to break up agglomerates 112' of the binder into sub-particles 112, if such agglomerates are present in the raw material source. Agitation also reduces the conductive particles 113' into smaller sub-particles 113, which are more suitable for adhesion relative to the AM particles 111. The mixing / agitation disclosed herein is sufficient to break up the interaction forces 401 between the agglomerates and also cause the binder 112 to adhere relative to the AM particles 111, wherein the bonding force 402 is greater than the separation force experienced by the electrostatic deposition system 200, thereby maintaining the morphology of the composite particles 101C and providing uniform deposition of the layer 252.

[0087] Figure 4 The sizes shown in are illustrative and are for example purposes only. In actual production, it is expected that the size of the binder sub-particles 112 will be between 0.1%-70% of the average size of the active material particles 111. When the average particle size of the active material is greater than 5 μm, it is beneficial if the average sub-particle size of the binder is less than 10% of the active material. When the average particle size of the active material is less than 5 μm, the preferred average sub-particle size of the binder is less than 70% of the active material.

[0088] It is expected that the granular feedstock 150 will exhibit different particle sizes, and a range of sizes is generally expected, which is normal. As long as the total range exhibits a typical distribution and average, abnormal particles outside the ranges described herein are unlikely to have a negative impact. As described above, similar distribution ranges are allowed for agglomerates and sub-particles; not all agglomerates / sub-particles can be expected to always break up strictly uniformly.

[0089] The sub-particle size of the conductive material is 1-100% of the average sub-particle size of the binder. The sub-particle size of the conductive material is preferably less than 30% of the average sub-particle size of the binder. From the perspective of the composition or component particles, not all of the binder 112 and the conductive particles 113 may adhere to the active material particles 111. In the electrode powder mixture, more than 50% by weight of the binder sub-particles should be attached to the surface of the active material particles. Preferably, more than 80% by weight of the binder sub-particles are attached to the surface of the active material particles. More than 50% by weight of the conductive sub-particles are attached to the surface of the binder sub-particles. And more than 50% of the binder conductive composite material particles are attached to the surface of the active material particles. Preferably, more than 80% by weight of the binder and the conductive material are attached to the surface of the active material particles.

[0090] If the composite electrode mix does not contain a conductive material, the binder sub-particles are directly attached relative to the surface of the active material particles.

[0091] Active material powder, binder powder and / or conductive material powder can be loaded and mixed in the mixer at the same time. In order to enable better crushing of binder and conductive agglomerates and increase the interaction between the sub-particles of binder and conductive material, it is preferred to pre-mix the binder and conductive material and then mix with the active material powder.

[0092] Some additional particle material size settings are as follows: The sub-particle size of the conductive material is 1-100% of the average sub-particle size of the binder. The sub-particle size of the conductive material is preferably less than 30% of the average sub-particle size of the binder.

[0093] In alternative arrangements, the method of attaching / adhering the binder / conductive particles relative to the active material particles is not limited to the dry powder mixing described herein. For example, in one exemplary embodiment, the binder / conductive material particles can be applied to the active material particles by mixing a suspension or solution of the binder / conductive material with the active material powder. In another exemplary embodiment, the binder particles can be coated on / relative to the surface of the active material particles by a spray drying method.

[0094] In a specific use case, mixer 130 uses a high shear mixer to stir the NCM / adhesive / CB powder mixture with a standard adhesive sub-particle size for electrostatic deposition. The high shear mixer provides a unique rotating mixing disk with a built-in eccentric mixing tool. The mixing speed in the range of 1 to 30m / s can be set to disperse and mix particles of different sizes. In this embodiment, an active material (NCM) with a size of about 10, a PVDF adhesive with a primary size of 200-300nm, and a conductive carbon with a primary size of 40-50nm are used. The AM / adhesive / CB particles with a weight ratio of 96:2:2 are mixed for 30 minutes using a high shear mixer. The SEM image of the mixed particles shows that CB and adhesive are coated on the AM surface.

[0095] Example

[0096] 1. Material Preparation and Electrode Preparation Using Electrostatic Spray Deposition

[0097] 700 g of a powder mixture containing heat-treated NMC, PVDF and carbon black (weight ratio of 90:7:3) was charged into a high shear mixer. Mixing studies were conducted with different mixing speeds and mixing times (sample 1: 12 m / s, 10 min; sample 3: 20 m / s, 20 min; sample 4: 25 m / s, 20 min).

[0098] The mixed NMC powder was loaded into the hopper of the electrostatic spray deposition system. The dry powder was fluidized by a carrier gas under vibration. The fluidized powder was charged by a corona electrostatic spray gun and deposited on a 15μm thick grounded Al foil. The coated side of the Al foil was pre-coated with a PVDF interfacial layer with a thickness of less than 1μm, which was applied using an electrostatic spray deposition technique. The deposited sample was placed in a hot plate and heated at a temperature of 250°C for about 1 hour to melt the binder. Finally, the annealed sample was pressed to the desired thickness using a roller press to achieve a porosity of 35%. The electrode sample can be used for SEM / EDS testing, adhesion testing, and electrochemical testing.

[0099] 2. SEM / EDS test of samples 1, 3 and 4

[0100] The mixed powder samples were analyzed by SEM / EDS to evaluate the deagglomeration of PVDF / carbon particles and the coating of PVDF / carbon on NMC particles. Figure 5A As shown in the figure, although a small amount of PVDF / carbon aggregates can be seen attached to the NMC surface, most of the NMC surface is exposed. The surface texture of NMC is clearly visible. This indicates that under the mixing of 12m / s and 10min, the surface of NMC is almost not covered by PVDF / carbon particles.

[0101] When the mixing intensity increased to 20 m / s, 20 min (sample 3; Figure 5B ) and 25m / s, 20min (sample 4, Figure 5C ), the surface of NMC particles is completely covered by PVDF / carbon.

[0102] Figures 6A-6C Sample 1 ( Fig. 6A )、Sample 3( Figure 6B ) and sample 4 ( Figure 6C ) is a larger area SEM image of the mixed powder.

[0103] The corresponding EDS results are shown in Fig. 7A Medium (sample 1; nickel mapping), Figure 7B (Sample 3; Ni mapping) and Figure 7C (Sample 4; Ni mapping), and in Fig. 8A Medium (sample 1; fluorine mapping), Figure 8B (Sample 3; Fluorine mapping) and Figure 8C (Sample 4; Fluorine mapping). ImageJ was used to process the elemental mapping images and eliminate the influence of signal intensity on image quality. The maximum intensity of each element was recorded in the image.

[0104] like Figures 7A-7C As shown, the distribution of nickel can be fully mapped onto the corresponding SEM images. The approximate shape of a single NMC particle is captured by nickel mapping. Fluorine mapping ( Figures 8A-8C) is an indication of the PVDF content, showing significant differences between the three hybrid materials.

[0105] From the fluorine mapping image mixed at 12m / s and 10min ( Fig. 8A ) The general spherical shape of the NMC particles is not visible in the mixed powder. This indicates that most of the PVDF particles are still randomly placed in the mixed powder rather than attached to the NMC particles. The tightly clustered black spots around the lower left corner of the image (indicated by the arrows) also indicate that some agglomerates of PVDF particles were not broken up under low-intensity mixing.

[0106] Fluorine begins to aggregate, indicating spherical NMC particles with higher mixing intensity, such as 20 m / s, 20 min (sample 3; Figure 8B ) and 25 m / s, 20 min (sample 4; Figure 8C ). 20m / s, 20min mixing (sample 3; Figure 8B ) of the fluorine map with tightly clustered black spots (indicated by arrows) around the left center (sample 3; Figure 8B ) indicates that PVDF particles are agglomerated in large quantities. Figure 6B From the corresponding SEM images in Figure 1, it can be seen that the NMC particles are located behind the large agglomerates of PVDF particles, but the PVDF agglomerates completely block the X-ray spectrum of nickel collected by the detector. Therefore, it appears as a vacancy (indicated by the arrow) in the corresponding nickel mapping image. No large PVDF agglomerates can be seen in the powder mixed at 25 m / s for 20 min (Sample 4). A relatively uniform distribution of PVDF particles is achieved, and from Figure 8C The corresponding fluorine mapping image can be seen in .

[0107] 3. Adhesion test

[0108] The bonding strength of the electrode was evaluated using a pull-off test. The electrode sample was cut into a disc with a diameter of 14.3 mm. The electrode disc was attached to a flat tip with a diameter of 12.7 mm using double-sided tape. The disc was attached to the substrate using double-sided tape with a compression force of 15 N, and then the maximum pull force that caused the disc to collapse was pulled and recorded. Fig. 9 is a graph showing the bonding strength of electrodes prepared by electrostatic spray deposition of powders (i.e., samples 1, 3, and 4) using different mixing times and speeds; Fig. 9 The graph shows that the samples prepared with longer mixing time showed better adhesion.

[0109] 4. EDS of electrodes Mapping

[0110] In another exemplary embodiment of the present disclosure, as described above, depolymerization of the binder particles is performed to form composite particles, and the composite particles are deposited on an aluminum foil substrate by electrostatic spray deposition, followed by hot calendering. This exemplary embodiment is characterized in that the composite particles in the electrode made of NCM 622 / PVDF / carbon have a carbon content of 20 mg / cm 2 The PVDF and carbon interact with the active particles to provide strong adhesion and conductivity.

[0111] like Fig.10 As shown in the SEM images of the nanostructured carbon nanotubes, the composite particles exhibited strong adhesion to the Al substrate.

[0112] like Fig.11 As shown in the EDS mapping images, the Ni active particles are uniformly distributed and adhered to the Al substrate.

[0113] like Fig.12 As shown in the EDS mapping image, the carbon particles are evenly distributed and adhered to the Ni active particles.

[0114] like Fig.13 As shown in the EDS mapping images, the PVDF binder particles are evenly distributed and adhered relative to the Ni active particles (based on imaging showing fluorine distribution).

[0115] 5. Mixed Research Results

[0116] A series of tests were conducted to determine the relationship between the mixing conditions associated with the formation of composite particles and the properties of those composite particles deposited on a substrate by ESD. A 700 g batch of powder mixture containing heat treated NMC, PVDF and carbon black (96:2:2 weight ratio) was loaded into a high shear mixer. Mixing studies were performed with different mixing speeds and mixing times. The resistance of the fabricated electrode thickness was measured on both sides by sandwiching the electrode disc between two measuring plates.

[0117] like Fig.14 As shown in the Figure 1, the resistance associated with the composite particles deposited on the substrate, which is a measure of the uniformity of the carbon distribution of the composite particles deposited on the substrate, shows that a favorable operating window is established at a mixing time of about 8 minutes to 35 minutes. Mixing times less than 8 minutes produced unacceptably high resistance levels (about 33 ohms). Significantly longer mixing times (about 50 minutes) did not produce improved results, but demonstrated approximately equivalent resistance performance compared to shorter duration mixing (e.g., about 30 minutes of mixing).

[0118] Go to Fig.15The bond strength associated with the composite particles deposited on the substrate, which is a measure of the uniformity and effectiveness of the binder distribution of the composite particles deposited on the substrate, indicates that a favorable operating window is established at a mixing time of about 8 minutes to 35 minutes - consistent with the above reference Fig.14 The operating window determined by the resistance measurements described is the same. Mixing times less than 8 minutes produced unacceptably low bond strengths. Significantly longer mixing times (about 50 minutes) did not produce improved results, but demonstrated roughly comparable average bond strengths compared to shorter duration mixing (e.g., about 30 minutes of mixing), as well as a wider range of performance.

[0119] based on Fig.14 and 15 The test results show that mixing times of about 8 minutes to about 35 minutes are effective for forming composite particles, demonstrating excellent distribution and maintained adhesion / attachment of the binder particles and conductive particles relative to the active particles according to the present invention.

[0120] The disclosed electrochemical energy storage devices may be incorporated into various assemblies / subassemblies, such as rechargeable lithium batteries, lithium-ion batteries, rechargeable lithium-sulfur batteries, solid-state batteries, rechargeable sodium batteries, and / or sodium-ion batteries.

[0121] While the systems and methods defined herein have been particularly shown and described with reference to embodiments thereof, it will be understood by those skilled in the art that various changes in form and details may be made therein without departing from the scope of the invention as encompassed by the appended claims.

Claims

1. An electrode, comprising: a conductive current collector substrate; one or more electrostatically deposited coatings deposited on and adhered relative to the conductive current collector substrate; wherein the one or more electrostatically deposited coatings include a plurality of dry-mixed composite particles, each dry-mixed composite particle of the plurality of dry-mixed composite particles including (i) one or more active material particles, and (ii) deagglomerated binder particles surrounding each of the one or more active material particles; and wherein the deagglomerated binder particles adhere relative to surfaces of active material particles of the one or more active material particles by interactions sufficient to withstand mixing associated with formation of the dry composite particles and overcome separation forces caused by deposition of one or more electrostatically deposited coatings on a conductive current collector substrate; The structure of the composite particles is thereby maintained when applied to a conductive current collector substrate.

2. The electrode according to claim 1, wherein the one or more active material particles are used as cathode material.

3. An electrode according to claim 2, wherein the one or more active material particles are selected from (i) lithium transition metal oxides, lithium transition metal sulfides, lithium polyanion cathode materials, including lithium transition metal phosphates, lithium transition metal silicates, or combinations thereof; or selected from (ii) sodium transition metal oxides, sodium polyanion cathode materials, Prussian blue analog cathode materials, or combinations thereof.

4. The electrode according to claim 1, wherein the one or more active material particles are used as an anode material.

5. The electrode according to claim 4, wherein the one or more active material particles are selected from (i) carbonaceous anode materials, graphite, Si, silicon-based composite materials, SiO x , lithium alloy materials, or lithium transition metal oxide anode materials, or combinations thereof; or selected from (ii) sodium alloy materials, or ion intercalation anode materials, including Prussian blue analogue anodes and sodium metal transition metal oxide anodes.

6. The electrode of claim 1, wherein the structure is incorporated into a component selected from the group consisting of a rechargeable lithium battery, a lithium ion battery, a rechargeable lithium sulfur battery, a solid state battery, a rechargeable sodium battery, and a sodium ion battery. 7 . The electrode according to claim 1 , wherein the depolymerized binder particles are formed of one or more of a polymer material, a polymer electrolyte, and a solid electrolyte composite material.

8. The electrode according to claim 7, wherein the polymer material is selected from polyvinylidene fluoride, polytetrafluoroethylene, polyethylene oxide, polymethyl methacrylate, polystyrene butadiene rubber binder, carboxymethyl cellulose binder, polyacrylic acid or a combination thereof.

9. The electrode of claim 1, wherein the dry-mixed composite particles further comprise conductive particles adhered to a surface of at least one of the one or more active material particles and the deagglomerated binder particles.

10. The electrode according to claim 9, wherein the conductive particles are selected from the group consisting of carbon black, carbon nanotubes, carbon fibers, graphene, graphite, or combinations thereof.

11. The electrode according to claim 1, wherein the conductive current collector substrate is selected from Al foil or Cu foil.

12. The electrode of claim 11, further comprising a primer layer to enhance adhesion between the one or more electrostatically deposited coatings and a conductive current collector substrate.

13. The electrode of claim 1, wherein the deagglomerated binder particles have a size that is 0.1% to 70% of the average size of the one or more active material particles.

14. The electrode of claim 1, wherein the average size of the one or more active material particles is greater than 5 μm, and the average size of the deagglomerated binder particles is less than 10% of the average size of the one or more active material particles.

15. The electrode of claim 1, wherein the average size of the one or more active material particles is greater than 5 Å, and the average size of the deagglomerated binder particles is less than 70% of the average size of the one or more active material particles.

16. The electrode of claim 1, wherein the dry-mixed composite particles further comprise conductive particles, and wherein greater than 50% of the deagglomerated binder particles and the conductive particles are adhered relative to the active material particles of the one or more active material particles.

17. A method of forming an electrode, comprising: combining the one or more active material particles and the deagglomerated binder particles to form a plurality of dry-mixed composite particles, wherein the deagglomerated binder particles surround each of the one or more active material particles; The plurality of dry-mixed composite particles are adhered to the surface of a conductive substrate by an electrostatic deposition process.

18. The method according to claim 17, further comprising: Agglomerates of the binder material are deagglomerated to form deagglomerated binder particles.

19. The method of claim 17, further comprising: combining conductive particles with the one or more active material particles and the deagglomerated binder particles, wherein the conductive particles adhere relative to surfaces of the deagglomerated binder particles, and Composite particles are then formed by adhering the combined binder and conductive particles to the surfaces of the one or more active material particles.

20. The method of claim 17, wherein the electrostatic deposition process is selected from the group consisting of corona charging electrostatic deposition, tribocharging electrostatic deposition, and direct electrode induction charging deposition.

21. The method of claim 17, wherein the deagglomerated binder particles are formed from a binder material by: combining one or more active material particles and a binder material, and agitating a dry mixture thereof to overcome agglomeration forces and forming deagglomerated binder particles from the binder material; thereby adhering the deagglomerated binder particles to the surface of the one or more active material particles to form composite particles, wherein the composite particles have sufficient interaction forces between the deagglomerated binder particles and the one or more active material particles to maintain adhesion during electrostatic charging, fluidization, and mechanical transport.

22. The method of claim 21, wherein the agitation generates sufficient force to pulverize the dry blend.

23. The method of claim 21, wherein adhering the plurality of dry-mixed composite particles relative to the surface of the conductive substrate comprises depositing the plurality of composite particles onto the conductive substrate to form a coating having a predetermined active material loading; and Further comprising densifying the coating and the conductive substrate by a densification process, wherein the densification process is selected from the group consisting of: (i) preheating the coating and the conductive substrate prior to the densification process, (ii) preheating the coating and the conductive substrate prior to densification under heating, and (iii) densifying the coating and the conductive substrate under heating.

24. The method of claim 23, wherein the densification process is repeated.

25. The method according to claim 21, wherein the agitation results in deagglomerated binder particles having a size between 200-1000 nm.

26. The method of claim 17, wherein the combining step comprises combining the conductive particles with one or more active material particles and deagglomerated binder particles to form a plurality of dry-mixed composite particles, whereby the conductive particles are adhered relative to the deagglomerated binder particles.

27. The method of claim 17, wherein the deagglomerated binder particles are formed from a binder material by: combining one or more active material particles and a binder material and agitating the dry blend thereof to overcome agglomeration forces and forming deagglomerated binder particles from the binder material; wherein the structure of the one or more active particles is maintained during agitation and adherence relative to the conductive substrate surface; wherein the deagglomerated binder particles are formed by deagglomerating agglomerates of a binder material; and Combining the one or more active material particles with the deagglomerated binder particles to form a plurality of dry-mixed composite particles comprises agitating the one or more active material particles and the deagglomerated binder particles in a solvent-free manner so that the deagglomerated binder particles adhere and maintain the morphology of the one or more active material particles during the agitation process.

28. The method of claim 17, further comprising: combining the deagglomerated binder particles with the conductive particles to adhere the conductive particles relative to the deagglomerated binder particles; and adhering the combined deagglomerated binder particles and conductive particles to the surface of each of the one or more active material particles to form dry-mixed composite particles, wherein the total amount of the conductive particles and the depolymerized binder particles in the dry-mixed composite particles is less than 20 wt %; wherein the average size of the binder particles is less than 50% of the average active material particle size; and The average size of the conductive particles is less than 30% of the average size of the deagglomerated binder particles.

29. The method of claim 17, further comprising forming an electrode from the conductive substrate to which the dry-mixed composite particles are adhered.

30. The method of claim 17, further comprising including the conductive substrate with the dry-mixed composite particles adhered thereto in a battery.

Citation Information

Patent Citations

  • Electrode for Energy Storage Device

    US20230246159A1