Multifunctional GO / MOF composite membrane as well as preparation method and application thereof
Through the composite of iron-based organic frame material and graphene oxide, a multifunctional GO/MOF composite film is formed, which solves the problems of low catalytic activity and intergranular defects of MOF film, and achieves efficient pollutant retention and photocatalytic degradation, which is suitable for industrial production .
Patent Information
- Application Number
- CN202411073220.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-01
AI Technical Summary
The existing MOF films have low catalytic activity and have intergranular defects, making it difficult to effectively intercept contaminants, and it is difficult to form a dense defect-free film through conventional processing techniques.
The composite of iron-based organic frame material and graphene oxide is adopted to form a multifunctional GO/MOF composite membrane through chelation and hydrogen bonding, which improves catalytic activity and molecular separation performance, and is quickly prepared by vacuum filtration.
It significantly improves the interception and catalytic performance of the MOF membrane, achieves high permeability, excellent molecular separation and photocatalytic degradation of pollutants, and has a simple and low-cost preparation process, which is suitable for industrial production.
Smart Images

Figure CN118874233A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of membrane separation, and in particular relates to a multifunctional GO / MOF composite membrane and a preparation method and application thereof. Background Art
[0002] At present, one of the biggest survival challenges facing the world's human beings is the shortage of water resources, and solving water pollution is the key to alleviating this problem. The emerging membrane separation technology has the advantages of high efficiency and energy saving in treating dye wastewater, organic wastewater and oily wastewater.
[0003] Metal-organic frameworks (MOFs) are porous crystalline materials with high surface area, pre-designed pore size, and uniformly dispersed active sites, consisting of metal cations or metal clusters and organic ligands. Their rich variety, high porosity, and precise pore structure regulation give them customization capabilities, which can be used to achieve precise and high-speed molecular screening for membrane separation. However, existing MOF membranes face many problems, such as low catalytic activity and intercrystalline defects that cannot effectively intercept pollutants. In addition, MOFs mainly exist in the form of fine powders or tiny particles. Due to the characteristics of the powders themselves, they are difficult to process into dense and defect-free membranes using conventional solvents and melt processing techniques.
[0004] To this end, the present invention is proposed. Summary of the invention
[0005] The main purpose of the present invention is to propose a multifunctional GO / MOF composite membrane and its preparation method and application. The preparation method of the multifunctional GO / MOF composite membrane in the present invention is simple to operate, and the reaction conditions are low-carbon and environmentally friendly. The retention and catalytic performance of the prepared multifunctional GO / MOF composite membrane are significantly improved.
[0006] In order to achieve the above objectives, the present invention provides the following technical solutions.
[0007] In a first aspect of the present invention, a method for preparing a multifunctional GO / MOF composite membrane is provided, which comprises the following steps:
[0008] The mixed solution of the iron-based organic framework material and graphene oxide is filtered onto the surface of the substrate membrane, and the multifunctional GO / MOF composite membrane is prepared by utilizing the chelation and hydrogen bonding between the iron-based organic framework material and the graphene oxide.
[0009] In some embodiments of the present invention, the iron-based organic framework material comprises a MIL-100 (Fe) material.
[0010] In some embodiments of the present invention, in the mixed solution, the mass ratio of the iron-based organic framework material to the graphene oxide is 50:(1-4).
[0011] In some embodiments of the present invention, the iron-based organic framework material is mixed with a graphene oxide solution and then subjected to ultrasonic treatment to obtain the mixed solution.
[0012] Preferably, the ultrasonic treatment time is 5 min to 6 min.
[0013] In some embodiments of the present invention, the preparation of the MIL-100 (Fe) material comprises the following steps:
[0014] The MIL-100 (Fe) material is prepared by mixing trimesic acid, ferric nitrate nonahydrate and deionized water and adjusting the pH of the solution to perform a crystallization reaction.
[0015] In some embodiments of the present invention, the preparation further comprises: washing and drying the material after the crystallization reaction to obtain the MIL-100 (Fe) material.
[0016] Preferably, the washing includes deionized water washing and solvent washing, the temperature of the deionized water washing is 60°C to 80°C, and the temperature of the solvent washing is 50°C to 70°C.
[0017] Preferably, the drying process is carried out at a temperature of 100° C. to 120° C. and for a time of 12 h to 14 h.
[0018] In some embodiments of the present invention, the pH value of the solution is 3-5.
[0019] Preferably, the pH adjusting agent employed comprises nitric acid.
[0020] In some embodiments of the present invention, the base film includes one of a cellulose acetate film, a nylon film, and a polytetrafluoroethylene film.
[0021] In a second aspect, the present invention provides a multifunctional GO / MOF composite membrane, wherein the multifunctional GO / MOF composite membrane is prepared by the preparation method described in the first aspect.
[0022] The third aspect of the present invention provides an application of the multifunctional GO / MOF composite membrane described in the second aspect or the multifunctional GO / MOF composite membrane prepared by the preparation method described in the first aspect in water purification.
[0023] Compared with the prior art, the present invention achieves the following technical effects:
[0024] 1. The present invention improves the molecular separation performance of the MOF membrane by modifying the MOF membrane with the flexible two-dimensional material graphene oxide as a filler, and at the same time improves the photocatalytic performance of the composite membrane.
[0025] 2. The multifunctional GO / MOF composite membrane provided by the present invention can be quickly prepared by vacuum filtration. The preparation process of the composite membrane is simple, does not require a large amount of organic solvent, is low in cost, and can be applied to large-scale industrial production.
[0026] 3. The multifunctional GO / MOF composite membrane provided by the present invention has at least three functions of high permeability, excellent molecular separation and photocatalytic degradation of pollutants.
[0027] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention, it can be implemented according to the contents of the specification. In order to make the above and other purposes, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are listed below. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Various other advantages and benefits will become apparent to those skilled in the art by reading the detailed description of the preferred embodiments below. The accompanying drawings are only used for the purpose of illustrating the preferred embodiments and are not to be considered as limiting the present invention. In the accompanying drawings:
[0029] Figure 1 is a process flow chart of a method for preparing a GO / MOF composite membrane according to some embodiments;
[0030] Figure 2 is a scanning electron microscope image of a GO / MOF composite membrane in some embodiments; wherein, Figure 2 a is GO obtained in Example 2 10 Surface image of / MIL-100(Fe) composite film; Figure 2 b is GO obtained in Example 1 40 Surface image of / MIL-100(Fe) composite film;
[0031] Figure 3 Graphs of pure water flux and water contact angle of GO / MOF composite membranes according to some embodiments; wherein, Figure 3 a is GO prepared in Examples 1 to 3 40 / MIL-100(Fe),GO 10 / MIL-100(Fe),GO 20 / water flux of MIL-100(Fe) membrane; Figure 3 b is GO prepared in Examples 1 to 3 40 / MIL-100(Fe),GO 10 / MIL-100(Fe),GO 20 / Water contact angle of MIL-100(Fe) composite film;
[0032] Figure 4The MIL-100 (Fe) film prepared in Comparative Example 1 and the GO prepared in Examples 1 to 3 40 / MIL-100(Fe),GO 10 / MIL-100(Fe),GO 20 / MIL-100(Fe) composite membrane for the retention of Coomassie Brilliant Blue (BBG);
[0033] Figure 5 The MIL-100 (Fe) film prepared in Comparative Example 1 and the GO prepared in Example 1 40 / Retention performance of MIL-100(Fe) composite membrane for four dye molecules;
[0034] Figure 6 is the photocatalytic performance and antifouling performance diagram of the membrane; among them, Figure 6 a is the MIL-100 (Fe) membrane in comparative example 1 and the GO in example 1 40 / Degradation efficiency of MIL-100(Fe) membrane on methylene blue (MB) within 40 min; Figure 6 b is the MIL-100 (Fe) film in Comparative Example 1 and the GO film in Example 1 40 / Flux recovery rate of MIL-100(Fe) membrane. DETAILED DESCRIPTION
[0035] The exemplary embodiments of the present invention will be described in more detail below with reference to specific embodiments. It should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided in order to enable a more thorough understanding of the present invention and to enable the scope of the present invention to be fully communicated to those skilled in the art.
[0036] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which the present invention belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention; the terms "including" and "having" in the specification and claims of the present invention and the above-mentioned figure descriptions and any variations thereof are intended to cover non-exclusive inclusions.
[0037] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present invention. The appearance of the phrase in various places in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0038] In the description of the embodiments of the present invention, the term "and / or" is only a description of the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B may represent: A exists, A and B exist at the same time, and B exists. In addition, the character " / " in this document generally indicates that the associated objects before and after are in an "or" relationship.
[0039] In the description of the embodiments of the present invention, the term "multiple" refers to more than two (including two). Similarly, "multiple groups" refers to more than two groups (including two groups), and "multiple pieces" refers to more than two pieces (including two pieces).
[0040] Metal-organic frameworks (MOFs) are porous crystalline materials with high surface area, pre-designed pore size, and uniformly dispersed active sites, consisting of metal cations or metal clusters and organic ligands. Their rich variety, high porosity, and precise pore structure regulation give them customization capabilities for precise and high-speed molecular screening for membrane separation. MOFs exist mainly in the form of fine powders or tiny particles, which are inherently brittle, insoluble, and non-thermoplastic, making them difficult to process into dense, defect-free films by conventional solvents and melt processing techniques. The problems faced by MOF photocatalytic films are mainly low catalytic activity and the fact that existing MOFs membranes have intercrystalline defects and cannot effectively intercept pollutants. Therefore, it is necessary to develop a dense, defect-free membrane that can improve the catalytic activity of MOFs.
[0041] Flexible graphene oxide (GO) has been widely studied as a two-dimensional sheet material with many advantages such as large specific surface area, amphiphilicity, good dispersibility and excellent proton transfer.
[0042] In order to enhance the separation performance and photocatalytic performance of the composite membrane, the present invention proposes a new method of using a small amount of GO and MOFs to composite to solve the defects of MOFs membrane.
[0043] At the same time, the present invention provides a dense multifunctional GO / MOF composite membrane with simple operation and low-carbon and environmentally friendly preparation process, so as to solve the problem that the MOF membrane surface has defects and poor catalytic performance in the existing preparation method.
[0044] The preparation method of the multifunctional GO / MOF composite membrane of the present invention is based on an iron-based MOF material with a photocatalytic function, namely a MIL-100 (Fe) material; the MIL-100 (Fe) material is added to a graphene oxide solution to obtain a uniformly mixed MIL-100 (Fe) / graphene oxide mixed solution; the MIL-100 (Fe) / graphene oxide mixed solution is filtered to the surface of a substrate membrane by a vacuum filtration method, and a GO / MOF composite membrane with a uniform structure is formed by utilizing the chelation and hydrogen bonding between MIL-100 (Fe) and graphene oxide.
[0045] The preparation method of the multifunctional GO / MOF composite membrane of the present invention specifically comprises the following steps:
[0046] (1) Preparation of MIL-100(Fe).
[0047] In an embodiment of the present invention, trimesic acid (H3BTC) and Fe(NO3)3·9H2O with a molar ratio of 0.66:1 are sequentially added to deionized water, and then HNO3 is added to adjust the pH value of the reaction system to 3-5. After sufficient stirring, the mixture is transferred into a 2L crystallization kettle, and the crystallization reaction is carried out at 180°C for 12 hours. After the crystallization is completed, the mixed solution is filtered to obtain an orange-yellow crude product.
[0048] To further remove unreacted H3BTC and Fe(NO3)3·9H2O, the samples were washed in hot deionized water at 60°C to 80°C and hot ethanol at 50°C to 70°C for 2.5 to 4 hours, respectively. The filtered solid samples were dried in an oven at 100°C to 120°C for 12 to 14 hours, and the final powdered product, MIL-100(Fe), was collected.
[0049] (2) Prepare MIL-100(Fe) / graphene oxide mixed solution.
[0050] In some embodiments of the present invention, MIL-100(Fe) is added to a graphene oxide solution to obtain a uniformly mixed MIL-100(Fe) / graphene oxide mixed solution.
[0051] In some embodiments of the present invention, after MIL-100(Fe) is added to the graphene oxide solution, ultrasonic treatment may be performed to obtain a uniformly dispersed photoresponsive molecular aggregate / graphene oxide mixed solution.
[0052] Specifically, the ultrasonic treatment time may be 5 min to 6 min.
[0053] In some embodiments of the present invention, in the MIL-100(Fe) / graphene oxide mixed solution, the mass ratio of MIL-100(Fe) to graphene oxide is 50:(1-4), for example, the mass ratio of MIL-100(Fe) to graphene oxide can be one of 50:1, 50:2, 50:3, 50:4 or any value satisfying the above range.
[0054] (3) Filtration.
[0055] In some embodiments of the present invention, the MIL-100(Fe) / graphene oxide mixed solution is filtered onto the surface of the substrate membrane by vacuum filtration, and a GO / MOF composite membrane with uniform structure is formed by chelation and hydrogen bonding between MIL-100(Fe) and graphene oxide.
[0056] In some embodiments of the present invention, the vacuum degree of the vacuum filtration method may be 1 bar.
[0057] In some embodiments of the present invention, the base film may be one of a cellulose acetate film, a nylon film, and a polytetrafluoroethylene film.
[0058] In some embodiments of the present invention, the pore size of the basement membrane may be 0.22 μm.
[0059] The GO / MOF composite membrane and the preparation method thereof in the present invention will be further described below in conjunction with specific embodiments; the materials and reagents used in the following embodiments, unless otherwise specified, can be commercially available products without limitation.
[0060] Example 1
[0061] Reference Figure 1 The preparation process shown is to prepare GO / MOF composite membrane.
[0062] (1) Trimellitic acid (H3BTC) and Fe(NO3)3·9H2O in a molar ratio of 0.66:1 were added to deionized water, and then HNO3 was added to adjust the pH value of the reaction system to 4. The molar ratio of HNO3 to Fe(NO3)3·9H2O was 1:4. After sufficient stirring, the mixture was transferred into a 2L reactor and crystallized at 180°C for 12 hours. After the crystallization was completed, the mixed solution was filtered to obtain an orange-yellow crude product.
[0063] To further remove unreacted H3BTC and Fe(NO3)3·9H2O, the samples were washed in hot deionized water at 70°C and hot ethanol at 65°C for 3 h, respectively. The filtered solid samples were dried in an oven at 120°C for 12 h, and then the final powdered product, MIL-100(Fe), was collected.
[0064] (2) The MIL-100(Fe) obtained in step (1) was fully dissolved in water to obtain a 0.5 mg / mL MIL-100(Fe) aqueous solution, and the MIL-100(Fe) aqueous solution was stored at room temperature.
[0065] (3) Take 500 μg of the MIL-100 (Fe) aqueous solution obtained in step (2) and 40 μg of graphene oxide (GO) and add them to 30 mL of water and ultrasonically treat for 5 min to mix them evenly to obtain a uniformly mixed GO 40 / MIL-100(Fe) mixed solution.
[0066] (4) The GO obtained in step (3) 40 The mixed solution of / MIL-100(Fe) was filtered onto the surface of an organic nylon membrane with a diameter of 47 mm and a pore size of 0.22 μm. After the filtration was completed, the formed GO 40 / MIL-100(Fe) composite membrane was stored in deionized water.
[0067] Example 2
[0068] Reference Figure 1 The preparation process shown is to prepare GO / MOF composite membrane.
[0069] (1) MIL-100(Fe) was prepared in the same manner as in Example 1.
[0070] (2) The MIL-100(Fe) obtained in step (1) was fully dissolved in water to obtain a 0.5 mg / mL MIL-100(Fe) aqueous solution, and the MIL-100(Fe) aqueous solution was stored at room temperature.
[0071] (3) Take 500 μg of the MIL-100 (Fe) aqueous solution obtained in step (2) and 10 μg of graphene oxide, add them to 30 mL of water and ultrasonically treat for 5 min to mix them evenly, to obtain a uniformly mixed GO 10 / MIL-100(Fe) mixed solution.
[0072] (4) The GO obtained in step (3) 10 The mixed solution of / MIL-100(Fe) was filtered onto the surface of an organic nylon membrane with a diameter of 47 mm and a pore size of 0.22 μm. After the filtration was completed, the formed GO 10 / MIL-100(Fe) composite membrane was stored in deionized water.
[0073] Example 3
[0074] Reference Figure 1 The preparation process shown is to prepare GO / MOF composite membrane.
[0075] (1) MIL-100(Fe) was prepared in the same manner as in Example 1.
[0076] (2) The MIL-100(Fe) obtained in step (1) was fully dissolved in water to obtain a 0.5 mg / mL MIL-100(Fe) aqueous solution, and the MIL-100(Fe) aqueous solution was stored at room temperature.
[0077] (3) Take 500 μg of the MIL-100 (Fe) aqueous solution obtained in step (2) and 20 μg of graphene oxide and add them to 30 mL of water for ultrasonic treatment for 5 min to mix them evenly to obtain a uniformly mixed GO 20 / MIL-100(Fe) mixed solution.
[0078] (4) The GO obtained in step (3) 20 The mixed solution of / MIL-100(Fe) was filtered onto the surface of an organic nylon membrane with a diameter of 47 mm and a pore size of 0.22 μm. After the filtration was completed, the formed GO 20 / MIL-100(Fe) composite membrane was stored in deionized water.
[0079] Comparative Example 1
[0080] (1) MIL-100(Fe) was prepared in the same manner as in Example 1.
[0081] (2) The MIL-100(Fe) obtained in step (1) was fully dissolved in water to obtain a 0.5 mg / mL MIL-100(Fe) aqueous solution, and the MIL-100(Fe) aqueous solution was stored at room temperature.
[0082] (3) 500 μg of the MIL-100(Fe) aqueous solution obtained in step (2) was added to 30 mL of water and ultrasonically treated for 5 min to mix evenly, thereby obtaining a uniformly mixed MIL-100(Fe) mixed solution.
[0083] (4) The MIL-100(Fe) mixed solution obtained in step (3) is filtered onto the surface of an organic nylon membrane with a diameter of 47 mm and a pore size of 0.22 μm. After the filtration is completed, the formed MIL-100(Fe) membrane is stored in deionized water.
[0084] The GO / MOF composite membranes prepared in Examples 1 to 3 and the MIL-100 (Fe) membrane prepared in the comparative example were characterized by wettability, membrane surface morphology, etc., and the pure water flux, the retention of dye molecules and the photocatalytic degradation function were detected and analyzed. The results are as follows: Figures 2 to 5 shown.
[0085] The water permeability of the prepared membrane was evaluated using standard terminal filtration equipment, including a nitrogen bottle, a digital balance, an ultrafiltration cup (MSC-50, MOSU China Co., Ltd.) and a computer. The quality of the filtrate was monitored using a digital balance at a pressure of 1.0 bar. The water flux was calculated using formula (1).
[0086]
[0087] In formula (1), J is the water flux (L m -2·h -1 bar -1 ), A is the effective membrane area (m 2 ), V is the filtrate volume (L), t is the filtration time (h), and P is the applied pressure (bar).
[0088] In the present invention, the retention capacity of each membrane was tested by filtering a 20 ppm dye solution. All samples were measured at least three times. The dye concentration in the feed and filtrate was analyzed using a UV-visible spectrophotometer. The retention rate was calculated according to formula (2).
[0089]
[0090] In formula (2), R is the retention rate, C0 and C1 are the dye concentrations before and after filtration, respectively.
[0091] In the present invention, the photocatalytic performance of the prepared film is evaluated by photocatalytic degradation of MB driven by visible light. The specific steps are as follows:
[0092] First, place the membrane face up so that it is fully exposed to visible light.
[0093] Then, 50 mL of MB solution (5 ppm) and 50 μL of H2O2 were added to the beaker; the solution was placed in the dark for 30 min to reach adsorption equilibrium and then exposed to visible light.
[0094] Subsequently, the changes in MB concentration were monitored by UV-visible spectroscopy every 5 min.
[0095] like Figure 2 a and Figure 2 As shown in b, with the increase of GO content, GO 40 A dense structure appears on the surface of the MIL-100(Fe) composite film.
[0096] like Figure 3 a and Figure 3 As shown in Figure b, with the increase of GO content, the permeability of the membrane gradually decreased, and the surface water contact angle of the membrane gradually increased. The pure water flux of MIL-100 (Fe) membrane was 2976.3 L·m -2 ·h -1 bar -1 , while GO 40 The pure water flux of the MIL-100(Fe) composite membrane decreased to 950.0 L·m -2 ·h -1 bar -1 .
[0097] The GO / MOF composite membranes prepared in Examples 1 to 3 and the MIL-100(Fe) membrane prepared in the comparative example were tested for separation performance and applied to the filtration separation of crystal violet (CrV), orange-yellow G (OY-G), Coomassie brilliant blue (BBG) and Congo red (CR).
[0098] like Figure 4 As shown, the retention rate of BBG by MIL-100 (Fe) membrane in Comparative Example 1 is 74.4%, and that of GO in Example 1 is 40 The rejection rate of BBG by the / MIL-100(Fe) composite membrane was 99.0%. 10 The rejection rate of BBG by the / MIL-100(Fe) composite membrane was 82.3%. 20 The rejection rate of BBG by the / MIL-100(Fe) composite membrane is 83.6%.
[0099] like Figure 5 As shown, the rejection rate of CR by MIL-100 (Fe) membrane in Comparative Example 1 is 85.1%, and that of GO in Example 1 is 40 The rejection rate of CR by the MIL-100(Fe) composite membrane is 99.8%.
[0100] The retention rate of CrV by MIL-100(Fe) membrane in Comparative Example 1 is 5.5%, and that of GO in Example 1 is 40 The rejection rate of CrV by the MIL-100(Fe) composite membrane is 21.6%.
[0101] Meanwhile, the GO / MOF composite films prepared in Examples 1 to 3 and the MIL-100 (Fe) film prepared in the comparative example were tested for their photocatalytic properties and applied to the degradation of MB.
[0102] like Figure 6 As shown in a, the degradation efficiency of MB by MIL-100 (Fe) membrane in Comparative Example 1 is 86.0% at 40 min. 40 The degradation efficiency of MB by / MIL-100(Fe) composite membrane was 94.0% in 40 min.
[0103] In addition, the GO / MOF composite membranes prepared in Examples 1 to 3 and the MIL-100 (Fe) membrane prepared in the comparative example were tested for their anti-pollution performance of BBG.
[0104] like Figure 6 As shown in b, the flux recovery rate of MIL-100 (Fe) in Comparative Example 1 is 85.9%, and that of GO in Example 1 is 40 The flux recovery rate of the / MIL-100(Fe) composite membrane was 94.1%.
[0105] In summary, the GO / MOF composite membrane provided by the present invention has at least three functions of high permeability, excellent molecular separation and photocatalytic degradation of pollutants.
[0106] The above is only a preferred specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the protection scope of the claims.
Claims
1. A method for preparing a multifunctional GO / MOF composite membrane, It is characterized in that The following steps are involved: The mixed solution of the iron-based organic framework material and graphene oxide is filtered onto the surface of the base film, and the multifunctional GO / MOF composite membrane is prepared by utilizing the chelation and hydrogen bonding between the iron-based organic framework material and the graphene oxide.
2. The method for preparing the multifunctional GO / MOF composite membrane according to claim 1, It is characterized in that The iron-based organic framework material includes MIL-100 (Fe) material.
3. The method for preparing the multifunctional GO / MOF composite membrane according to claim 1 or 2, It is characterized in that In the mixed solution, the mass ratio of the iron-based organic framework material to the graphene oxide is 50:(1-4).
4. The method for preparing the multifunctional GO / MOF composite membrane according to claim 1, It is characterized in that The iron-based organic framework material is mixed with a graphene oxide solution and then subjected to ultrasonic treatment to obtain the mixed solution; Preferably, the ultrasonic treatment time is 5 min to 6 min.
5. The method for preparing the multifunctional GO / MOF composite membrane according to claim 2, It is characterized in that The preparation of the MIL-100 (Fe) material comprises the following steps: The MIL-100 (Fe) material is prepared by mixing trimesic acid, ferric nitrate nonahydrate and deionized water and adjusting the pH of the solution to perform a crystallization reaction.
6. The method for preparing the multifunctional GO / MOF composite membrane according to claim 5, It is characterized in that The preparation further comprises: washing and drying the material after the crystallization reaction to obtain the MIL-100 (Fe) material; Preferably, the washing includes deionized water washing and solvent washing, the temperature of the deionized water washing is 60°C to 80°C, and the temperature of the solvent washing is 50°C to 70°C; Preferably, the drying process is carried out at a temperature of 100° C. to 120° C. and for a time of 12 h to 14 h.
7. The method for preparing the multifunctional GO / MOF composite membrane according to claim 5, It is characterized in that The pH value of the solution is 3 to 5; Preferably, the pH adjusting agent employed comprises nitric acid.
8. The method for preparing the multifunctional GO / MOF composite membrane according to claim 1, It is characterized in that The base film includes one of a cellulose acetate film, a nylon film, and a polytetrafluoroethylene film.
9. A multifunctional GO / MOF composite membrane, It is characterized in that The multifunctional GO / MOF composite membrane is prepared by the preparation method described in any one of claims 1 to 8.
10. Use of the multifunctional GO / MOF composite membrane according to claim 9 or the multifunctional GO / MOF composite membrane prepared by the preparation method according to any one of claims 1 to 8 in water purification.