Self-healing-chlorine fixation-corrosion inhibition hybrid microcapsule and preparation method thereof
By designing the combination of self-healing-chlorine-inhibiting hybrid microcapsules, capsule wall and capsule core, the problems of slow repair process and Cl-permeability in the existing technology are solved, and the rapid self-healing and long-term effect of the coating is achieved Anti-corrosion to ensure the stable operation of marine equipment.
Patent Information
- Application Number
- CN202410919737.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing self-healing microcapsule materials are not repaired quickly enough in complex marine environments, and corrosive ions such as Cl- can still penetrate, resulting in coating aging and metal corrosion, which cannot meet the long-term service needs, and lacks coating/metal interfaces. Effective protection of corrosion.
Design a self-healing-solid chlorine-inhibiting hybrid microcapsule. The capsule wall consists of synthetic cellulose and layered double hydroxide nanosheets. The nanosheets are inserted with anion corrosion inhibitors, and the capsule core is single-component dry Oil repair agents are prepared by co-precipitation method and solvent evaporation method. They have the functions of self-healing, chlorine solidification and corrosion inhibition, capture chloride ions and release corrosion-resilient factors, and synergistically enhance efficiency.
It realizes rapid self-healing and long-term anti-corrosion of the coating, prevents the diffusion of chloride ions, inhibits corrosion of the coating/metal interface, extends the coating life, and ensures the stable operation of marine equipment.
Smart Images

Figure CN118874353A_ABST
Abstract
Description
Technical field:
[0001] The present invention belongs to the technical field of intelligent anti-corrosion materials, and specifically relates to a self-healing-chlorine-fixing-corrosion inhibition hybrid microcapsule and a preparation method thereof, which is suitable for long-term corrosion protection of metal structures and equipment in complex marine environments. Background technology:
[0002] Marine engineering and equipment that have been in service for a long time in complex marine environments face serious corrosion problems. Coating protection technology is the most economical and effective means of anti-corrosion for marine engineering and equipment. Among them, polymer coatings such as epoxy resins and polyurethanes have always been the most commonly used anti-corrosion coating systems for marine engineering and equipment due to their many advantages such as low price, stable structure, excellent mechanical properties, good corrosion resistance, and convenient construction. However, under the influence of complex service conditions and multi-factor coupled environments: natural environmental aging such as high temperature, high humidity, high salinity, and strong ultraviolet radiation, as well as external force damage such as mechanical impact and scratches, it is very easy to produce some micro defects such as micropores and micro cracks inside and on the surface of the coating. If these micro defects are not repaired in a timely and effective manner, the barrier effect of the coating to corrosive media will be weakened. - Corrosive ions such as ions gradually invade the coating through micro-defects, causing the polymer chains to swell and break, accelerating coating aging and shortening the coating's service life. When the corrosive medium further penetrates into the coating / metal interface, local corrosion will occur in the metal structure, reducing its strength, posing a great threat to the safe and stable operation of marine engineering and equipment.
[0003] In response to the problem of microcrack damage in polymer coatings, researchers have developed a series of self-healing microcapsule materials. The microcapsule materials coated with the repair agent are embedded in the polymer coating. When microcracks appear in the coating, the microcapsules rupture under the action of the cracks and release the repair agent. Under the action of capillaries, the repair agent penetrates into the cracks, undergoes a cross-linking reaction, achieves self-healing of the microcracks, and restores the integrity of the coating. For example, a method for preparing a self-warning and self-repairing coating disclosed in Chinese Patent 202410225144.0 includes the following steps: Step 1, adding a fluorescent probe, a polyphenol-type glycidyl ether epoxy resin, and a polyurethane prepolymer to hexyl acetate, mixing and dispersing them to obtain a microcapsule core solution A; adding a corrosion inhibitor molecule, a curing agent, and a polyurethane prepolymer to hexyl acetate, mixing and dispersing them to obtain a microcapsule core solution B; Step 2, mixing water, a polyethylene-maleic anhydride aqueous solution, urea, resorcinol, and ammonium chloride, and adjusting the pH to maintain at 3 to obtain a solution. Liquid A, two portions of solution A are prepared; after the microcapsule core solution A is mixed and emulsified with one portion of solution A, a formaldehyde aqueous solution is added, and microcapsules are polymerized to obtain microcapsules A; after the microcapsule core solution B is mixed and emulsified with another portion of solution A, a formaldehyde aqueous solution is added, and microcapsules are polymerized to obtain microcapsules B; step three, microcapsules A, microcapsules B, hexyl acetate, resin, and polyoxypropylene triamine are blended until microcapsules A and microcapsules B are completely dispersed, and coated on a substrate to obtain a self-warning and self-repairing dual-functional coating based on a pH-responsive aggregation-induced fluorescent probe. A self-healing coating disclosed in Chinese patent 202311833270.6 includes a self-healing polyurethane and a self-healing microcapsule doped in the self-healing polyurethane, wherein the mass ratio of the self-healing microcapsule to the self-healing polyurethane is 1:2-4, the average particle size of the self-healing microcapsule is 1-10 μm, and the self-healing microcapsule is a double-shell self-healing microcapsule; the double-shell self-healing microcapsule includes a hexamethylene diisocyanate trimer core material, a polystyrene inner shell layer and a polyurethane outer shell layer from the inside to the outside, the coverage rate of the self-healing microcapsule is more than 80%, and the core material loading rate is More than 40%, the preparation method of the self-healing coating comprises the following steps: mixing self-healing polyurethane and triethylamine, performing salt-forming reaction, and obtaining a salt-forming compound; the mass ratio of the self-healing polyurethane and triethylamine is 8 to 16:1; mixing the salt-forming compound and water to obtain a viscous self-healing polyurethane; mixing the viscous self-healing polyurethane and a self-healing microcapsule solution to obtain a self-healing coating slurry; coating and drying the self-healing coating slurry in sequence to obtain the self-healing coating, the temperature of the salt-forming reaction is 40 to 50°C, and the time is 30 to 40 minutes.Chinese Patent No. 201910681195.3 discloses a method for preparing a self-healing coating material, which includes the following steps: 1) Preparation of wall material: melamine, thiourea and formaldehyde are added to the reactor in sequence, stirred evenly, adjusted to pH 8.5, and kept in a constant temperature water bath, and then graphene oxide particles are added, ultrasonically dispersed, and the wall material is obtained for standby use; 2) Preparation of modified epoxy resin: silane coupling agent, epoxy resin and catalyst are added to the reactor in sequence, stirred evenly, kept in a constant temperature water bath, and modified epoxy resin is obtained for standby use; 3) Preparation of core material: emulsifier and distilled water are added to the reactor in sequence, stirred at high speed Until the emulsifier is dissolved, the modified epoxy resin is added into the reactor, and the defoamer is added, and the core material is obtained by stirring at room temperature; 4) Preparation of modified microcapsules: Add the wall material into the core material, stir evenly at high speed, adjust the pH to 3.3, slowly heat up to 70°C, stir for 1h, adjust the pH to 7, cool, vacuum filter, wash with deionized water and acetone, dry at 50°C to constant weight, obtain modified microcapsules, and set aside; 5) Preparation of self-healing coating: Mix epoxy resin varnish with polyetheramine curing agent, add modified microcapsules, add leveling agent and defoamer, stir at room temperature, and obtain self-healing coating. However, when the self-healing microcapsule materials in the above patents and prior art are used in polymer coatings, the repair process is not completed instantaneously, and it takes several hours or even days to achieve steady state or maximum repair. Therefore, during the coating repair process, Cl. - The corrosive ions will continue to penetrate into the coating through the coating defects. In addition, after the repair is completed, the Cl - It will also cause corrosion of the metal matrix, and the generated corrosion products will accumulate at the coating / metal interface, affecting the adhesion of the coating. In severe cases, it will cause problems such as coating peeling and shedding. Based on this, the microcapsule material can only repair the microcrack damage of the coating, which is difficult to meet the long-term service requirements of the marine anti-corrosion coating. - The ability to capture corrosive ions such as chlorine and the ability to self-repair the corrosion reaction at the coating / metal interface are particularly important. Therefore, it is urgent to develop a microcapsule material that integrates self-healing, chlorine fixation and corrosion inhibition. Through the synergistic effect of the multi-functions, the long-term stable and reliable service of the coating can be achieved, making up for the shortcomings of the existing self-repairing microcapsule materials with single functions and limited repair effects. Summary of the invention:
[0004] The purpose of the present invention is to overcome the shortcomings of the prior art, develop and design a hybrid microcapsule that integrates self-healing, chlorine fixation and corrosion inhibition functions, and improve the intelligent protection level of marine anti-corrosion coatings through the synergistic effect of the functions of hybrid microcapsules, providing multi-level corrosion protection for marine metal structures.
[0005] In order to achieve the above-mentioned purpose, the present invention relates to a self-healing-chlorine-fixing-corrosion inhibition hybrid microcapsule consisting of a capsule wall and a capsule core, which is prepared by a coprecipitation method and a solvent evaporation method, wherein the capsule wall is composed of a hybrid of synthetic cellulose and layered double hydroxide (LDH) nanosheets, and the capsule core is a single-component dry oil repair agent;
[0006] Among them, the layered double hydroxide sheets are loaded with anionic corrosion inhibitors, have good anion exchange properties, can capture chloride ions in the environment, and simultaneously release corrosion inhibitors.
[0007] The process of the preparation method of a self-healing-chlorine-fixing-corrosion inhibition hybrid microcapsule disclosed by the present invention comprises two steps: synthesizing MgAl-LDH nanosheets loaded with corrosion inhibition factors by a coprecipitation method and synthesizing MgAl-LDH hybrid microcapsules by a solvent evaporation method. By adjusting the amount of MgAl-LDH nanosheets loaded with corrosion inhibition factors, the amount of capsule cores, the stirring speed or the concentration of an emulsifier and other process parameters, self-healing-chlorine-fixing-corrosion inhibition hybrid microcapsules with different particle sizes and different coverage rates are obtained; specifically:
[0008] (1) Preparation of MgAl-LDH nanosheets loaded with corrosion inhibitors
[0009] First, Mg(NO3)2·6H2O and Al(NO3)3·9H2O were added to boiling deionized water, and heated and stirred to obtain a mixed solution No. 1;
[0010] Add sodium hydroxide and corrosion inhibitor into boiling deionized water, stir and dissolve while heating to obtain mixed solution No. 2;
[0011] Under stirring and high-purity nitrogen protection conditions, adding the mixed solution No. 2 dropwise into the mixed solution No. 1 to obtain a mixed solution No. 3;
[0012] Among them, the molar ratio of Mg(NO3)2·6H2O to Al(NO3)3·9H2O in the mixed solution No. 1 is 2:1, and the total concentration of metal salts is 0.1-0.2 mol / L;
[0013] The concentration of NaOH in the No. 2 mixed solution is 0.1-0.5 mol / L, and the corrosion inhibitor is an inorganic corrosion inhibitor having good corrosion inhibition effect on metal materials such as carbon steel, magnesium alloy, aluminum alloy, etc., including sodium tungstate, sodium molybdate, and sodium metavanadate;
[0014] Then, the pH value of the No. 3 mixed solution is adjusted by a 2 mol / L NaOH aqueous solution, reacted at high temperature, cooled to room temperature for aging, and a corrosion inhibitor-loaded MgAl-LDH nanosheet slurry is obtained;
[0015] The pH value of the No. 3 mixed solution is 10-11, the temperature of the high temperature reaction is 80-100°C, the time is 4-8h, and the aging time is 12h;
[0016] Finally, the corrosion inhibitor-loaded MgAl-LDH nanosheet slurry is centrifuged, the supernatant is removed, the remaining slurry is washed with deionized water, and then centrifuged again, and the washing-centrifugation is repeated for multiple times, and then dried to obtain the corrosion inhibitor-loaded MgAl-LDH nanosheet;
[0017] (2) Preparation of MgAl-LDH hybrid microcapsules:
[0018] First, a stabilizer is added to deionized water, and mechanically stirred at room temperature until completely dissolved, and then a capsule core material and an emulsifier are added respectively, and mechanical stirring is continued to emulsify the capsule core material to obtain a capsule core emulsion;
[0019] The mass of the stabilizer is 2-5g, including gelatin and gum arabic, the mass of deionized water is 100-1000g, the mass of the capsule core material is 10-50g, including tung oil and linseed oil, the molecular structure contains unsaturated double bonds, it is easy to oxidize and dry in the air to form an elastic and flexible solid film, and it is cheap, easy to obtain, and environmentally friendly. The mass of the emulsifier is 0.1-1g, including polyvinyl alcohol, sodium dodecylbenzene sulfonate, and OP-10, the emulsification temperature is 25-35°C, the rotation speed is 400-800r / min, and the time is 0.5-2h;
[0020] Then, the capsule wall material is fully dissolved in an organic solvent, and the MgAl-LDH nanosheet powder loaded with the corrosion inhibitor is added, and mechanical stirring is performed to obtain a capsule wall mixed solution;
[0021] The mass of the capsule wall material is 5-20g, which is synthetic cellulose, including methyl cellulose, ethyl cellulose, and carboxymethyl cellulose, and has good film-forming properties; the mass of the organic solvent is 100-500g, including dichloromethane and 1,2-dichloroethane; the mass of the MgAl-LDH nanosheet loaded with the corrosion inhibition factor is 1-10g;
[0022] Finally, the capsule wall mixture is slowly poured into the capsule core emulsion, mechanically stirred at room temperature, the capsule wall covers the capsule core, the solvent is evaporated, solidified, impurities are removed, rinsed, and dried to obtain MgAl-LDH hybrid microcapsules;
[0023] The coating rotation speed is 400-800 r / min, the time is 1-5 h, the curing time is 0.5-2 h, the temperature is 40-60° C., and the drying temperature is 60-120° C., and the time is 12-24 h.
[0024] Compared with the prior art, the present invention is hybridized by a magnesium aluminum layered double hydroxide (MgAl-LDH) loaded with a corrosion inhibition factor and a microcapsule coated with a repair agent, and is prepared by a coprecipitation method and a solvent evaporation method. The MgAl-LDH is hybridized in the microcapsule wall in the form of a surface load, and the microcapsule core is coated with a dry oil single-component repair agent, which has multiple functions of self-healing, chlorine fixation, and corrosion inhibition. After being added to an organic coating, when the organic coating is damaged, the capsule wall cracks and releases the repair agent, and the repair agent undergoes a self-oxidation reaction under oxygen-containing conditions to form a high molecular polymer to heal microcracks in the coating. At the same time, the MgAl-LDH with excellent interlayer anion exchange performance captures chloride ions in the corrosive medium, prevents the chloride ions from diffusing inside the coating, and simultaneously releases corrosion-inhibiting anions, thereby inhibiting the electrochemical reaction of the corrosion site at the coating / metal interface. The long-term corrosion protection of the organic coating is achieved through the synergistic effect of self-healing, chlorine fixation, and corrosion inhibition, and the operating stability of marine equipment can be guaranteed. Description of the drawings:
[0025] Figure 1 This is a process flow chart of the preparation of the self-healing-chlorine-fixing-corrosion inhibition hybrid microcapsules involved in Example 1 of the present invention.
[0026] Figure 2 This is a graph showing the self-healing performance test results of the self-healing-chlorine-fixing-corrosion inhibition hybrid microcapsules prepared in Example 1 of the present invention.
[0027] Figure 3 This is a graph showing the chlorine-fixing performance test results of the self-healing-chlorine-fixing-corrosion inhibition hybrid microcapsules prepared in Example 1 of the present invention.
[0028] Figure 4 This is a graph showing the corrosion inhibition performance test results of the self-healing-chlorine-fixing-corrosion inhibition hybrid microcapsules prepared in Example 1 of the present invention. Specific implementation method:
[0029] The present invention will be further described below in conjunction with the accompanying drawings and specific implementation methods.
[0030] Embodiment 1:
[0031] The specific process flow of the method for preparing a self-healing-chlorine-fixing-corrosion inhibition hybrid microcapsule involved in this embodiment is as follows: Figure 1 As shown:
[0032] First, coprecipitation
[0033] Add 2.56 g of Mg(NO3)2·6H2O and 1.88 g of Al(NO3)3·9H2O to 100 mL of boiling deionized water, and heat and stir to dissolve to obtain mixed solution No. 1;
[0034] Add 1.2 g of sodium hydroxide and 2.42 g of Na2MoO4·2H2O into 100 mL of boiling deionized water, and stir to dissolve while heating to obtain a mixed solution No. 2;
[0035] Under stirring and high-purity nitrogen protection conditions, the No. 2 mixed solution was added dropwise to the No. 1 mixed solution through a peristaltic pump for 30 minutes to obtain a No. 3 mixed solution;
[0036] The pH value of the mixed solution No. 3 was adjusted to 11 by using a 2 mol / L NaOH aqueous solution, reacted at 80°C for 6 h, cooled to room temperature and aged for 12 h, to obtain a MgAl-LDH nanosheet slurry loaded with molybdate anions;
[0037] Then, hybridization
[0038] 3 g of gelatin was added to 1000 mL of deionized water, and mechanically stirred at room temperature until completely dissolved. Then, 20 g of tung oil and 1 g of sodium dodecylbenzene sulfonate were added respectively, and mechanically stirred at a temperature of 30° C. and a rotation speed of 600 r / min for 30 min of emulsification to obtain a capsule core emulsion.
[0039] 15 g of ethyl cellulose was fully dissolved in 200 g of dichloromethane, and 2 g of MgAl-LDH nanosheet powder loaded with molybdate anions was added, and mechanical stirring was performed at a temperature of 30° C. for 30 min to obtain a capsule wall mixture;
[0040] Finally, the solvent evaporates
[0041] The capsule wall mixture is poured into the capsule core emulsion, and mechanically stirred at a speed of 600 r / min at room temperature to allow the capsule wall to coat the capsule core for 3 hours to obtain microcapsules, which are then kept at a temperature of 50° C. for 1 hour to solidify the microcapsules, remove wall material impurities and broken microcapsules suspended on the liquid surface, and rinse the microcapsules with deionized water;
[0042] The microcapsules were placed in a drying oven at 60°C for 24 hours to obtain self-healing-chlorine-fixing-corrosion inhibition hybrid microcapsules;
[0043] The preparation method of the molybdate anion-loaded MgAl-LDH nanosheet powder is as follows:
[0044] First, the MgAl-LDH nanosheet slurry loaded with molybdate anions was centrifuged and the supernatant was removed;
[0045] Then, the remaining MgAl-LDH nanosheet slurry loaded with molybdate anions was washed with deionized water, centrifuged, and washed and centrifuged three times to obtain a white slurry;
[0046] Finally, the white slurry was placed in an oven at 60° C. and dried for 24 h to obtain MgAl-LDH nanosheet powder loaded with molybdate anions.
[0047] Embodiment 2:
[0048] This example involves the self-healing performance test of the self-healing-chlorine-fixing-corrosion inhibition hybrid microcapsules prepared in Example 1:
[0049] The self-healing-chlorine-fixing-corrosion-inhibiting hybrid microcapsules prepared in Example 1 were added to the polymer anticorrosion coating by mechanical blending, with the mass proportion of the self-healing-chlorine-fixing-corrosion-inhibiting hybrid microcapsules being 1%. After mechanical stirring for 30 minutes, the coating was applied to the surface of the metal substrate by manual brushing, and after curing at room temperature for 24 hours, it was cured at 50° C. for 24 hours.
[0050] After the coating is cured, an artificial defect with a length of 2 mm, a width of 0.3 mm and a depth to the metal substrate is made on the coating surface with a scalpel. The self-healing process of the defect is monitored in an atmospheric environment using the micro-area scanning Kelvin probe technique to verify the self-healing performance of the coating by the self-healing-chlorine-fixing-corrosion inhibition hybrid microcapsules.
[0051] The results are as follows Figure 2 As shown in the figure, after the coating was scratched, the initial maximum ΔV value was about 1.15V. The surface defects were tested for the second and third time at intervals of 5h. The scratch became significantly narrower after the second test and basically disappeared after the third test. At the same time, the maximum ΔV values also dropped to 0.77V and 0.52V respectively. The scanning Kelvin probe mainly reveals the surface state changes by measuring the lateral differences in the surface work function. The lower potential difference (ΔV) indicates that the sample surface has better integrity.
[0052] It can be seen that the self-healing-chlorine-fixing-corrosion inhibition hybrid microcapsules have excellent self-healing ability. However, even so, achieving complete healing of defects is actually a time-consuming process. The corrosive medium will have enough time to penetrate into the surface of the metal matrix before the defects are completely repaired, thereby causing metal corrosion. Therefore, it is of great significance that the self-healing-chlorine-fixing-corrosion inhibition hybrid microcapsules also have corrosion inhibition function.
[0053] Embodiment 3:
[0054] This example involves the chlorine-fixing performance test of the self-healing-chlorine-fixing-corrosion-inhibiting hybrid microcapsules prepared in Example 1:
[0055] 5 g of the self-healing-chlorine-fixing-corrosion-inhibiting hybrid microcapsules prepared in Example 1 were added to 100 mL of a 3.5 wt.% NaCl aqueous solution, and ultrasonically dispersed. After soaking for 6 hours, the mixture was centrifuged and separated. The mixture was rinsed with a large amount of deionized water for multiple times. After drying, the surface of the self-healing-chlorine-fixing-corrosion-inhibiting hybrid microcapsules was subjected to elemental analysis by an energy spectrometer to verify the chlorine-fixing performance of the self-healing-chlorine-fixing-corrosion-inhibiting hybrid microcapsules.
[0056] The results are as follows Figure 3 As shown in the figure, compared with the surface element analysis results of the self-healing-chlorine-fixing-corrosion inhibition hybrid microcapsules before immersion, the Mo element signal of the self-healing-chlorine-fixing-corrosion inhibition hybrid microcapsules after immersion basically disappeared, and a new Cl element signal appeared, indicating that the Cl in the electrolyte - Participated in the ion exchange process, on the one hand, Cl - Initiated LDH interlayer MoO4 2- On the other hand, Cl - The self-healing-chlorine-fixing-corrosion-inhibiting hybrid microcapsules are retained in the LDH layer, indicating that the self-healing-chlorine-fixing-corrosion-inhibiting hybrid microcapsules have good chlorine-fixing performance.
[0057] Embodiment 4:
[0058] This example involves the sustained release performance test of the self-healing-chlorine-fixing-corrosion inhibition hybrid microcapsules prepared in Example 1:
[0059] The self-healing-chlorine-fixing-corrosion-inhibiting hybrid microcapsules prepared in Example 1 were added to the polymer anticorrosion coating by mechanical blending, with the mass proportion of the self-healing-chlorine-fixing-corrosion-inhibiting hybrid microcapsules being 1%. After mechanical stirring for 30 minutes, the coating was applied to the surface of the metal substrate by manual brushing, and after curing at room temperature for 24 hours, it was cured at 50° C. for 24 hours.
[0060] After the coating is cured, a fine needle tip is used to create a defect point with a diameter of 300-500 μm on the coating surface, exposing the metal substrate under the coating to the corrosive medium: 0.1M NaCl aqueous solution. Scanning vibrating electrode technology is used to conduct micro-area corrosion electrochemical testing to verify the corrosion inhibition performance of the self-healing-chlorine-fixing-corrosion inhibition hybrid microcapsules.
[0061] The results are as follows Figure 4 As shown in Figure 2, after immersion for 0.5 h, the maximum anodic current density at the coating defect is about 45 μA / cm 2 , and dropped to the noise level after 4 hours, indicating that the corrosion reaction at the coating / metal interface was effectively suppressed, confirming that the self-healing-chlorine-fixing-corrosion inhibition hybrid microcapsules have a high efficiency in corrosion inhibition.
[0062] Embodiment 5:
[0063] This embodiment relates to the application of the self-healing-chlorine-fixing-corrosion-inhibiting hybrid microcapsules prepared in Example 1 in a polymer-based anticorrosive coating;
[0064] The metal substrate is made of Q235 steel. Before use, the surface oxide film, rust and burrs are removed by shot blasting, and the surface oil is removed by cleaning.
[0065] The polymer coating is a commercially available bisphenol A epoxy resin;
[0066] The coating thickness after curing is 100±10μm.
Claims
1. A self-healing-chlorine-fixing-corrosion inhibition hybrid microcapsule, characterized in that: It consists of a capsule wall and a capsule core. The capsule wall is a hybrid of synthetic cellulose and layered double hydroxide nanosheets, and the capsule core is a single-component dry oil repair agent.
2. The self-healing-chlorine-fixing-corrosion-inhibiting hybrid microcapsule according to claim 1, characterized in that: Prepared by co-precipitation and solvent evaporation.
3. A method for preparing self-healing-chlorine-fixing-corrosion inhibition hybrid microcapsules, characterized in that: The corrosion inhibitor-loaded MgAl-LDH nanosheets were firstly synthesized by co-precipitation method, and then the MgAl-LDH hybrid microcapsules were synthesized by solvent evaporation method.
4. The method for preparing a self-healing-chlorine-fixing-corrosion inhibition hybrid microcapsule according to claim 3, characterized in that: The specific process is: (1) Preparation of MgAl-LDH nanosheets loaded with corrosion inhibitors First, Mg(NO3)2·6H2O and Al(NO3)3·9H2O were added to boiling deionized water, and heated and stirred to obtain a mixed solution No. 1; Add sodium hydroxide and corrosion inhibitor into boiling deionized water, stir and dissolve while heating to obtain mixed solution No. 2; Under stirring and high-purity nitrogen protection conditions, adding the mixed solution No. 2 dropwise into the mixed solution No. 1 to obtain a mixed solution No. 3; Then, the pH value of the No. 3 mixed solution is adjusted by a 2 mol / L NaOH aqueous solution, reacted at high temperature, cooled to room temperature for aging, and a corrosion inhibitor-loaded MgAl-LDH nanosheet slurry is obtained; Finally, the corrosion inhibitor-loaded MgAl-LDH nanosheet slurry is centrifuged, the supernatant is removed, the remaining slurry is washed with deionized water, and then centrifuged again, and the washing-centrifugation is repeated for multiple times, and then dried to obtain the corrosion inhibitor-loaded MgAl-LDH nanosheet; (2) Preparation of MgAl-LDH hybrid microcapsules: First, a stabilizer is added to deionized water, and mechanically stirred at room temperature until completely dissolved, and then a capsule core material and an emulsifier are added respectively, and mechanical stirring is continued to obtain a capsule core emulsion; Then, the capsule wall material is dissolved in an organic solvent, and the MgAl-LDH nanosheet powder loaded with the corrosion inhibitor is added, and mechanical stirring is performed to obtain a capsule wall mixed solution; Finally, the capsule wall mixture is poured into the capsule core emulsion, mechanically stirred at room temperature, the solvent is evaporated, solidified, impurities are removed, rinsed, and dried to obtain MgAl-LDH hybrid microcapsules, namely self-healing-chlorine-fixing-corrosion inhibition hybrid microcapsules.
5. The method for preparing a self-healing-chlorine-fixing-corrosion inhibition hybrid microcapsule according to claim 4, characterized in that: In step (1): The molar ratio of Mg(NO3)2·6H2O to Al(NO3)3·9H2O in mixed solution No. 1 is 2:1, and the total concentration of metal salts is 0.1-0.2 mol / L; The concentration of NaOH in the No. 2 mixed solution is 0.1-0.5 mol / L, and the corrosion inhibitor is an inorganic corrosion inhibitor, including sodium tungstate, sodium molybdate, and sodium metavanadate; The pH value of the No. 3 mixed solution is 10-11, the temperature of the high-temperature reaction is 80-100°C, the time is 4-8h, and the aging time is 12h.
6. The method for preparing a self-healing-chlorine-fixing-corrosion inhibition hybrid microcapsule according to claim 4, characterized in that: In step (2): The mass of the stabilizer is 2-5g, including gelatin and gum arabic, the mass of deionized water is 100-1000g, the mass of the capsule core material is 10-50g, including tung oil and linseed oil, the mass of the emulsifier is 0.1-1g, including polyvinyl alcohol, sodium dodecylbenzene sulfonate, and OP-10, the emulsification temperature is 25-35°C, the rotation speed is 400-800r / min, and the time is 0.5-2h; The mass of the capsule wall material is 5-20 g, which is synthetic cellulose, including methyl cellulose, ethyl cellulose, and carboxymethyl cellulose; the mass of the organic solvent is 100-500 g, including dichloromethane and 1,2-dichloroethane; the mass of the MgAl-LDH nanosheet loaded with the corrosion inhibition factor is 1-10 g; The coating rotation speed is 400-800r / min, the time is 1-5h, the curing time is 0.5-2h, the temperature is 40-60℃, the drying temperature is 60-120℃, and the time is 12-24h.
7. A method for preparing self-healing-chlorine-fixing-corrosion inhibition hybrid microcapsules according to any one of claims 4 to 6, characterized in that: By adjusting the amount of MgAl-LDH nanosheets loaded with corrosion inhibition factors, the amount of capsule cores, the stirring speed or the emulsifier concentration, self-healing-chlorine-fixing-corrosion inhibition hybrid microcapsules with different particle sizes and different coverage rates can be obtained.
Citation Information
Patent Citations
Magnesium alloy micro-arc oxidation electrolyte and preparation method thereof and magnesium alloy surface treatment method
CN110241452A
Chlorine fixation-self-healing synergistic anti-corrosion microcapsule and preparation method thereof
CN115010400A
Magnesium alloy super-hydrophobic and active protection difunctional composite anticorrosive coating and preparation method thereof
CN115433477A
Dual self-repairing anticorrosive coating and preparation method thereof
CN115433478A
Chlorine-force triggered multifunctional corrosion inhibition microcapsule and preparation method thereof
CN115784655A
Cited By
Connector surface composite coating and preparation process thereof
CN120830139A
A connector surface composite coating and a process for making the same
CN120830139B
Microcapsule composite coating resistant to chlorine corrosion and capable of preventing marine organism fouling and preparation method
CN121759021A