Preparation method and application of carbon-supported vulcanized nano zero-valent iron
By using activated carbon-loaded, vulcanized, modified carbon-based vulcanized nano zero-valent iron (SnZVI-AC) in the soil, the problem of removing antibiotic resistance genes in the soil is solved, and the efficient, stable and environmentally friendly ARGs removal effect is achieved, reducing the effect of reducing the The risk of secondary pollution.
Patent Information
- Application Number
- CN202411009552.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-01
AI Technical Summary
The prior art is difficult to effectively remove antibiotic resistance genes (ARGs) in soil, and traditional methods have problems such as saturation of adsorbents, high equipment costs and secondary pollution in water treatment, making it difficult to deal with the removal of gene pollutants in soil.
Using activated carbon as a carrier, the adsorption performance of ARGs is improved by loading and vulcanizing the modified carbon-based vulcanized nano zero-valent iron (SnZVI-AC), and the adsorption performance of ARGs is improved by electrostatic action and micropore filling, thereby reducing the environmental abundance of ARGs.
It improves the adsorption efficiency of ARGs and the stability of materials, extends the service life, reduces the risk of secondary pollution, and provides an efficient, stable and environmentally friendly genetic pollutant removal solution in soil.
Smart Images

Figure CN118874397A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of soil treatment, and in particular to a preparation method and application of carbon-supported sulfide nano zero-valent iron. Background Art
[0002] Antibiotics are widely used to treat bacterial diseases in humans and animals due to their ability to inhibit or kill bacteria. However, antibiotics and antibiotic resistance genes (ARGs) are highly mobile and biotoxic, and a considerable portion (about 30%-90%) of antibiotic use is not absorbed by organisms, but is excreted into the environment with feces and urine, forming wastewater and soil containing antibiotics and their metabolites.
[0003] Most of the existing technologies are for the treatment of genetic pollutants in water bodies. At present, the treatment of antibiotics in wastewater mainly includes adsorption, advanced oxidation and biological methods. Among them, the adsorption method uses porous materials as adsorbents to achieve wastewater treatment by adsorbing antibiotics through porous materials; however, during the adsorption process, the adsorbent is easily saturated, and the adsorbent will not only adsorb antibiotics, but also adsorb other substances in the wastewater, so a large amount of adsorbent is required. At the same time, the regeneration of the adsorbent is also a problem that limits its application. Advanced oxidation methods mainly include Fenton method and modified Fenton method, activated persulfate, photoelectrocatalysis, etc., with high reagent, energy consumption and equipment costs, and will cause subsequent pollution problems. Biological methods treat pollutants through anaerobic digestion. Anaerobic digestion is a sustainable development technology for sewage treatment, with the advantages of low sludge production, low energy consumption and high biogas production, and occupies an important position in sewage treatment plants. However, various studies have shown that antibiotics in wastewater themselves have antibacterial and bactericidal effects, which will seriously affect the normal growth and metabolism of microorganisms in anaerobic systems. In an environment of antibiotic stress, it is still unknown whether anaerobic digestion can effectively remove antibiotic resistance genes. Overall, the effect of removing antibiotic resistance genes is not ideal and may even promote their spread.
[0004] Chinese patent CN 110776081 A provides a method for removing antibiotic resistance genes in livestock and poultry wastewater, comprising the following steps: adding copper sulfate pentahydrate to hot water at 35-45°C, stirring until the copper sulfate pentahydrate is dissolved, then adding iron powder to the solution, continuing to stir until the solution turns reddish brown, standing, pouring out the supernatant, and obtaining nano copper cluster particles; taking livestock and poultry wastewater, heating it to 23-27°C, maintaining it for 4-10 minutes, then adding the nano copper cluster particles prepared in step (1) thereto, stirring for 20-50 minutes. This method has the advantages of high removal efficiency, low removal cost, short removal time, simple operation, and no secondary pollution.
[0005] Chinese patent CN 104671618 B discloses a coagulation method for removing antibiotic resistance genes in sewage, which mainly removes antibiotic resistance genes in sewage by adding two coagulants, polyaluminium chloride (PACl) and polyferric sulfate (PFS), to the grid effluent and secondary effluent, providing a reliable idea for eliminating the pollution of antibiotic resistance genes in sewage.
[0006] Most existing technologies focus on methods to remove genetic pollutants from water bodies. However, soil is one of the environments with the richest microbial diversity and is therefore the main repository of ARGs, especially in agricultural soils where organic fertilizers and recycled water are applied. Compared with traditional pollutants, the removal of ARGs is more challenging. Even in the absence of antibiotic selection pressure, ARGs can spread in microbial communities to offspring and non-resistant bacteria through vertical and horizontal gene transfer. Therefore, it is urgent to develop a material that can remove genetic pollutants in soil.
[0007] Nano zero-valent iron (nZVI) has the characteristics of small size, strong reducibility, and large specific surface area, and is one of the most widely studied nanomaterials. However, due to its own magnetism, it is easy to agglomerate and oxidize. It is very difficult to modify nZVI. The specific modification methods include coating, loading, sulfidation, etc. The outer surface of sulfided nano zero-valent iron (S-nZVI) is covered with a layer of sulfide, which can not only improve the dispersion performance of nanoparticles, but also effectively inhibit the hydrogen evolution process of nZVI. However, SnZVI is often used as a catalyst for Fenton reaction to degrade ARGs, and the effect of simply using it as an adsorbent to adsorb pollutants is not ideal. Carbon-based materials are often used as supporting materials for nZVI. Activated carbon (AC) has the characteristics of porosity and high specific surface area. SnZVI can be loaded on the surface or pores of porous materials. While playing a dispersing role, it can also use the adsorption capacity of porous materials to adsorb ARGs on the surface, providing SnZVI with adsorption efficiency.
[0008] Based on this, the present invention provides a method for preparing carbon-based sulfide nano zero-valent iron and its application in removing ARGs, to provide a new idea for removing ARGs using nanomaterials and to provide an effective method for reducing the environmental risks of ARGs. Summary of the invention
[0009] In view of the above problems, the present invention provides a method for preparing carbon-based sulfide nano zero-valent iron. The method uses activated carbon as a matrix and is modified by nZVI loading and sulfide reduction. After application, the method can reduce the absolute abundance of total ARGs in the environment mainly through electrostatic action and supplemented by micropore filling, thereby increasing its adsorption performance for ARGs.
[0010] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0011] In one aspect, the present invention provides a method for preparing carbon-supported sulfided nano-zero-valent iron, comprising the following steps:
[0012] S1: NaBH 4 and Na 2 S 2 O 4 and mixed with a solvent to obtain a mixed solution 1; wherein NaBH 4 The concentration of Na in the mixed solution is 0.25-0.29 mol / L. 2 S 2 O 4 The concentration is 0.03-0.034mol / L;
[0013] S2: Activated carbon and FeSO 4 7H 2 O solution is mixed, mixed solution 1 is added, stirred to make it sulfurized, washed, and dried to obtain carbon-based sulfurized nano zero-valent iron;
[0014] The Na 2 S 2 O 4 S and FeSO 4 7H 2 The molar ratio of Fe in O is 0.4-0.6:1;
[0015] The FeSO 4 7H 2 The mass ratio of iron in O to activated carbon is 1:1-3.
[0016] Preferably, the solvent described in S1 is water; further preferably, the solvent described in S1 is selected from at least one of deionized water, distilled water and purified water; more preferably, the solvent described in S1 is deionized water.
[0017] Preferably, NaBH 4 The concentration is 0.26-0.28mol / L;
[0018] Further preferably, the NaBH 4 The concentration is 0.27-0.28 mol / L;
[0019] More preferably, the mixed solution described in S1 contains NaBH 4 The concentration is 0.275-0.28mol / L.
[0020] Preferably, Na in the mixed solution described in S1 2 S 2 O 4The concentration is 0.03-0.035mol / L;
[0021] Further preferably, Na in the mixed solution described in S1 2 S 2 O 4 The concentration is 0.033-0.035mol / L.
[0022] Preferably, the mixing in S2 is stirring, and the stirring time is 30-50 min;
[0023] More preferably, the stirring time is 40 min.
[0024] Preferably, S2 is performed under a nitrogen atmosphere.
[0025] Preferably, the stirring time in S2 is 1-1.5h, and the stirring speed is 700-900r / min;
[0026] More preferably, the stirring time in S2 is 1 h, and the stirring speed is 800 r / min.
[0027] Preferably, the Na 2 S 2 O 4 S and FeSO 4 7H 2 The molar ratio of Fe in O is 0.5:1;
[0028] Preferably, the FeSO 4 7H 2 The mass ratio of iron in FeSO to activated carbon is 1:1 or 1:3; further preferably, the FeSO 4 7H 2 The mass ratio of iron in O to activated carbon is 1:1.
[0029] Preferably, the cleaning described in S2 is to clean the precipitate obtained by sulfidation with ethanol and water respectively;
[0030] Preferably, the water is deionized water.
[0031] Preferably, the volume ratio of ethanol to water is 1:0.9-1.1; further preferably, the volume ratio of ethanol to water is 1:1.
[0032] Preferably, the specific operation of freeze drying described in S2 is: drying under vacuum conditions of -52°C-60°C for 10-12h.
[0033] On the other hand, the present invention provides the use of the carbon-supported sulfide nano zero-valent iron in treating genetic pollutants in soil.
[0034] Preferably, the soil is selected from at least one of brown soil or red soil; further preferably, the soil is brown soil and red soil, the brown soil is I and the red soil is U.
[0035] Compared with the prior art, the present invention has the following beneficial effects:
[0036] 1. The carbon-based sulfide nano zero-valent iron prepared by the present invention using activated carbon loading and sulfurization modification has excellent antioxidant and corrosion resistance. It retains the functional groups and hydrophilicity of activated carbon while also having the magnetic properties of carbon-based sulfide nano zero-valent iron.
[0037] 2. The present invention uses activated carbon fiber as a carrier to significantly improve the dispersibility and stability of sulfided nano zero-valent iron. The structure of this composite material makes nZVI particles more evenly dispersed, reduces agglomeration, thereby increasing the surface area in contact with pollutants and improving removal efficiency. At the same time, sulfidation treatment can also alleviate the oxidation problem of nZVI and extend the service life of the material.
[0038] 3. The SnZVI-AC of the present invention has good reusability, which is important for reducing long-term operating costs and improving economic feasibility. Reduced risk of secondary pollution: Compared with the use of nZVI or other heavy metal removal technologies alone, SnZVI-AC reduces the risk of secondary pollution through its unique structure and functional modification, especially when treating high-concentration wastewater.
[0039] 4. It fills the gap in the existing technology for removing genetic pollutants in soil and provides an efficient, stable and environmentally friendly solution. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 The figure shows the adsorption effect of different loading substrates on salmon sperm (simulating ARGs);
[0041] Figure 2 The adsorption effect diagram of the products of the embodiment and comparative example on salmon sperm (simulated ARGs); Figure 3 The pore size distribution diagrams of nZVI, SnZVI, AC, and SnZVI-AC-1;
[0042] Figure 4 TEM images of SnZVI, AC, and SnZVI-AC-1: b is the TEM image of AC, and c is the TEM image of SnZVI-AC-1;
[0043] Figure 5 SEM images of SnZVI-AC-1 and SnZVI-AC-2: a is the SEM image of SnZVI-AC-1, b is the SEM image of SnZVI-AC-2;
[0044] Figure 6 XRD patterns of SnZVI-AC, SnZVI, nZVI and AC;
[0045] Figure 7 Kinetic models for AC, SnZVI, SnZVI-AC-1, and SnZVI-AC-2;
[0046] Figure 8 Isotherm models for AC, SnZVI, SnZVI-AC-1, and SnZVI-AC-2;
[0047] Fig. 9 XRD patterns of SnZVI-AC applied into red soil or brown soil;
[0048] Fig.10 FTIR spectrum of SnZVI-AC applied to red soil or brown soil;
[0049] Fig.11 The abundance changes of sul1, tetA and ermF after adding different amounts of materials into brown soil and red soil, a is the abundance change of sul1, b is the abundance change of tetA, and c is the abundance change of ermF;
[0050] Note: Figure 1 , 2 Different letters in 11 indicate significant differences between different groups or conditions. The significant differences were analyzed by one-way ANOVA test using IBM SPSS Statistics 26. DETAILED DESCRIPTION
[0051] In order to make the technical means, creative features, purpose and effect of the present invention easy to understand, the present invention is further explained below in conjunction with specific embodiments, but the following embodiments are only preferred embodiments of the present invention, not all. Based on the embodiments in the implementation mode, other embodiments obtained by those skilled in the art without making creative work all belong to the protection scope of the present invention. It is worth noting that the raw materials used in the present invention are all common commercial products, and their sources are not specifically limited. The technology and scientific terms used in the embodiments have the meanings commonly understood by those of ordinary skill in the art to which the present invention belongs.
[0052] Glossary:
[0053] AC: Activated Carbon
[0054] SnZVI: Sulfided Nano-Zero-Valent Iron
[0055] SnZVI-AC: Carbon-based sulfide nano-zero-valent iron
[0056] SnZVI-AC-1: Carbon-based sulfide nano zero-valent iron (Fe / C=1:1)
[0057] SnZVI-AC-2: Carbon-based sulfide nano zero-valent iron (Fe / C=1:3)
[0058] Example 1
[0059] The method for preparing carbon-based sulfide nano zero-valent iron of the present invention comprises the following steps:
[0060] (1) NaBH preparation 4 and Na 2 S 2 O 4 Mixed solution: 2.1 g NaBH 4 and 0.5795 g Na 2 S 2 O 4 Place in a beaker and add 250 mL of pure water to dissolve to obtain NaBH 4 and Na 2 S 2 O 4 The mixture contains NaBH 4 The concentration is 0.2775mol / L, Na 2 S 2 O 4 The concentration is 0.033285 mol / L.
[0061] (2) 0.7435 g of activated carbon and 3.7 g of FeSO 4 7H 2 O was placed in a 1L three-necked flask, 200mL of pure water solution was added, and stirred for 30min under nitrogen. Then, after stirring evenly, 250mL of NaBH 4 and Na 2 S 2 O 4 The mixed solution was stirred at the same speed for 1 hour after the addition was completed to allow it to be fully sulfurized. The black solid precipitate in the suspension was washed and collected with anhydrous ethanol and deionized water, respectively, and then freeze-dried under vacuum conditions at -52°C to obtain carbon-based sulfurized nano zero-valent iron, marked as SnZVI-AC 1:1-0.5. SnZVI-AC-1 was used instead of SnZVI-AC 1:1-0.5 in subsequent experimental results.
[0062] The Na 2 S 2 O 4 S and FeSO 4 7H2 The molar ratio of Fe in O is 0.5, and the FeSO 4 7H 2 The mass ratio of iron in O to activated carbon is 1:1.
[0063] Example 2
[0064] Compared with Example 1, the only difference is that the amount of activated carbon added in step (2) is 2.2359 g, and the carbon-based sulfide nano zero-valent iron is obtained, marked as SnZVI-AC 1:3-0.5. SnZVI-AC-2 is used instead of SnZVI-AC 1:3-0.5 in the subsequent experimental results.
[0065] The Na 2 S 2 O 4 S and FeSO 4 7H 2 The molar ratio of Fe in O is 0.5, and the FeSO 4 7H 2 The mass ratio of iron in O to activated carbon is 1:3.
[0066] The remaining operations are the same as those in Example 1.
[0067] Comparative Example 1
[0068] Compared with Example 1, the only difference is that the amount of activated carbon added in step (2) is 3.265 g, and the carbon-based sulfide nano zero-valent iron is obtained, which is marked as SnZVI-AC 1:5-0.5.
[0069] The Na 2 S 2 O 4 S and FeSO 4 7H 2 The molar ratio of Fe in O is 0.5, and the FeSO 4 7H 2 The mass ratio of iron in O to activated carbon is 1:5.
[0070] The remaining operations are the same as those in Example 1.
[0071] Comparative Example 2
[0072] Compared with Example 1, the only difference is that no activated carbon is added in step (2), and carbon-based sulfide nano zero-valent iron is obtained, which is marked as SnZVI-AC-0.5.
[0073] The Na 2 S 2 O 4 S and FeSO 4 7H2 The molar ratio of Fe in O is 0.5.
[0074] The remaining operations are the same as those in Example 1.
[0075] Comparative Example 3
[0076] Compared with Example 1, the only difference is that in step (1), Na 2 S 2 O 4 The added amount was 0.3477 g to prepare carbon-based sulfide nano zero-valent iron, marked as SnZVI-AC 1:1 -0.3.
[0077] The Na 2 S 2 O 4 S and FeSO 4 7H 2 The molar ratio of Fe in O is 0.3. 4 7H 2 The mass ratio of iron in O to activated carbon is 1:1.
[0078] The remaining operations are the same as those in Example 1.
[0079] Comparative Example 4
[0080] Compared with Example 1, the only difference is that in step (1), Na 2 S 2 O 4 The amount of added is 0.3477 g, the amount of activated carbon added in step (2) is 2.2359 g, and carbon-based sulfide nano zero-valent iron is prepared, marked as SnZVI-AC 1:3-0.3.
[0081] The Na 2 S 2 O 4 S and FeSO 4 7H 2 The molar ratio of Fe in O is 0.3. 4 7H 2 The mass ratio of iron in O to activated carbon is 1:3.
[0082] The remaining operations are the same as those in Example 1.
[0083] Comparative Example 5
[0084] Compared with Example 1, the only difference is that in step (1), Na 2 S 2 O 4The amount of added is 0.3477 g, the amount of activated carbon added in step (2) is 3.265 g, and carbon-based sulfide nano zero-valent iron is prepared, marked as SnZVI-AC 1:5 -0.3.
[0085] The Na 2 S 2 O 4 S and FeSO 4 7H 2 The molar ratio of Fe in O is 0.3. 4 7H 2 The mass ratio of iron in O to activated carbon is 1:5.
[0086] The remaining operations are the same as those in Example 1.
[0087] Comparative Example 6
[0088] Compared with Example 1, the only difference is that in step (1), Na 2 S 2 O 4 The amount of addition was 0.3477 g, and no activated carbon was added in step (2), and carbon-based sulfide nano zero-valent iron was obtained, which was marked as SnZVI-AC-0.3.
[0089] The Na 2 S 2 O 4 S and FeSO 4 7H 2 The molar ratio of Fe in O is 0.3.
[0090] The remaining operations are the same as those in Example 1.
[0091] Comparative Example 7
[0092] Compared with Example 1, the only difference is that in step (1), Na 2 S 2 O 4 The added amount was 1.1590 g to prepare carbon-based sulfide nano zero-valent iron, marked as SnZVI-AC 1:1 -1.
[0093] The Na 2 S 2 O 4 S and FeSO 4 7H 2 The molar ratio of Fe in O is 1, and the FeSO 4 7H 2 The mass ratio of iron in O to activated carbon is 1:1.
[0094] The remaining operations are the same as those in Example 1.
[0095] Comparative Example 8
[0096] Compared with Example 1, the only difference is that in step (1), Na 2 S 2 O 4 The amount of added is 1.1590 g, the amount of activated carbon added in step (2) is 2.2359 g, and carbon-based sulfide nano zero-valent iron is prepared, marked as SnZVI-AC 1:3-1.
[0097] The Na 2 S 2 O 4 S and FeSO 4 7H 2 The molar ratio of Fe in O is 1, and the FeSO 4 7H 2 The mass ratio of iron in O to activated carbon is 1:3.
[0098] The remaining operations are the same as those in Example 1.
[0099] Comparative Example 9
[0100] Compared with Example 1, the only difference is that in step (1), Na 2 S 2 O 4 The amount of added is 1.1590 g, the amount of activated carbon added in step (2) is 3.265 g, and carbon-based sulfide nano zero-valent iron is prepared, marked as SnZVI-AC 1:5 -1.
[0101] The Na 2 S 2 O 4 S and FeSO 4 7H 2 The molar ratio of Fe in O is 1, and the FeSO 4 7H 2 The mass ratio of iron in O to activated carbon is 1:5.
[0102] The remaining operations are the same as those in Example 1.
[0103] Comparative Example 10
[0104] Compared with Example 1, the only difference is that in step (1), Na 2 S 2 O 4 The amount of addition was 1.1590 g, and no activated carbon was added in step (2), and carbon-based sulfide nano zero-valent iron was obtained, which was marked as SnZVI-AC-3.
[0105] The Na 2 S2 O 4 S and FeSO 4 7H 2 The molar ratio of Fe in O is 1.
[0106] The remaining operations are the same as those in Example 1.
[0107] Comparative Example 11
[0108] Compared with Example 1, the only difference is that in step (1), Na 2 S 2 O 4 The added amount was 0.1159 g to prepare carbon-based sulfide nano zero-valent iron, marked as SnZVI-AC 1:1 -0.1.
[0109] The Na 2 S 2 O 4 S and FeSO 4 7H 2 The molar ratio of Fe in O is 0.1, and the FeSO 4 7H 2 The mass ratio of iron in O to activated carbon is 1:1.
[0110] The remaining operations are the same as those in Example 1.
[0111] Comparative Example 12
[0112] Compared with Example 1, the only difference is that in step (1), Na 2 S 2 O 4 The amount of added is 0.1159 g, the amount of activated carbon added in step (2) is 2.2359 g, and carbon-based sulfide nano zero-valent iron is prepared, marked as SnZVI-AC 1:3-0.1.
[0113] The Na 2 S 2 O 4 S and FeSO 4 7H 2 The molar ratio of Fe in O is 0.1, and the FeSO 4 7H 2 The mass ratio of iron in O to activated carbon is 1:3.
[0114] The remaining operations are the same as those in Example 1.
[0115] Comparative Example 13
[0116] Compared with Example 1, the only difference is that in step (1), Na 2 S 2 O4 The amount of added is 0.1159 g, the amount of activated carbon added in step (2) is 3.265 g, and carbon-based sulfide nano zero-valent iron is prepared, marked as SnZVI-AC 1:5-0.1.
[0117] The Na 2 S 2 O 4 S and FeSO 4 7H 2 The molar ratio of Fe in O is 0.1, and the FeSO 4 7H 2 The mass ratio of iron in O to activated carbon is 1:5.
[0118] The remaining operations are the same as those in Example 1.
[0119] Comparative Example 14
[0120] Compared with Example 1, the only difference is that in step (1), Na 2 S 2 O 4 The amount of addition was 0.1159 g, and no activated carbon was added in step (2), and carbon-based sulfide nano zero-valent iron was obtained, which was marked as SnZVI-AC-0.1.
[0121] The Na 2 S 2 O 4 S and FeSO 4 7H 2 The molar ratio of Fe in O is 0.1.
[0122] The remaining operations are the same as those in Example 1.
[0123] Table 1. Parameter comparison of Examples 1-2 and Comparative Examples 1-14
[0124] Example Molar ratio of S / Fe Fe / C mass ratio Example 1 0.5 1:1 Example 2 0.5 1:3 Comparative Example 1 0.5 1:5 Comparative Example 2 0.5 / Comparative Example 3 0.3 1:1 Comparative Example 4 0.3 1:3 Comparative Example 5 0.3 1:5 Comparative Example 6 0.3 / Comparative Example 7 1 1:1 Comparative Example 8 1 1:3 Comparative Example 9 1 1:5 Comparative Example 10 1 / Comparative Example 11 0.1 1:1 Comparative Example 12 0.1 1:3 Comparative Example 13 0.1 1:5 Comparative Example 14 0.1 /
[0125] Test Example 1
[0126] Screening of load base and material ratio:
[0127] Using salmon sperm DNA as a model DNA, the adsorption capacity of montmorillonite, kaolin, zeolite, nanoapatite, biochar, activated carbon, graphene, and carbon nanotubes on DNA was investigated (e.g. Figure 1 As shown, Figure 1Different letters in the table indicate significant differences between different groups or conditions. The significant differences were analyzed by one-way ANOVA test using IBM SPSS Statistics 26.) Batch adsorption experiments showed that activated carbon, multi-walled carbon nanotubes, and graphene had high adsorption capacities for DNA, reaching 62.75 and 63.82 mg / g, respectively. However, considering that multi-walled carbon nanotubes and graphene are relatively expensive and difficult to prepare, activated carbon is the most suitable choice as the loading substrate for SnZVI.
[0128] The products prepared in Examples 1-2 and Comparative Examples 1-14 were investigated for their adsorption to salmon sperm DNA ( Figure 2 , Figure 2 Different letters in the table indicate significant differences between groups or conditions. The significant differences were analyzed by one-way ANOVA test using IBM SPSS Statistics 26. Figure 2 As shown in the figure, the original SnZVI has limited adsorption capacity for salmon sperm DNA, and the adsorption capacity is the highest when S / Fe=1, reaching only 22.54 mg / g. After SnZVI is loaded with AC, its adsorption capacity is significantly improved, which is 6.47 times that of SnZVI, but with the increase of the amount of AC loaded, its adsorption capacity begins to decrease. This phenomenon occurs in SnZVI-AC with different S / Fe. Taking S / Fe=0.5 as an example, when Fe / C increases from 1:1 to 1:3, its adsorption capacity decreases by 19.48 mg / g; when Fe / C increases from 1:1 to 1:5, its adsorption capacity decreases by 41.87 mg / g. This may be because the appropriate amount of AC will improve the dispersibility of SnZVI and increase the adsorption sites, but excessive AC will also form agglomerations, which is not conducive to the loading and adsorption of SnZVI. Therefore, Fe / C=1:1 and 1:3 are selected as the best loading ratios of SnZVI-AC. At the same Fe / C, when S / Fe increases from 0.1 to 0.3, the adsorption of SnZVI-AC increases by 20.64mg / g-30.01mg / g; when S / Fe increases from 0.3 to 5, the adsorption of SnZVI-AC increases by 22.37mg / g-28.83mg / g; but when S / Fe increases from 0.5 to 1, the adsorption of SnZVI-AC decreases by 22.43mg / g-25.26mg / g. Theoretically, the higher the S / Fe of SnZVI, the more iron sulfides on its surface, but the internal Fe 0 Therefore, the optimal ratio of SnZVI-AC was determined to be S / Fe=0.5, Fe / C=1:1.
[0129] Test Example 2
[0130] SnZVI-AC-1 and SnZVI-AC-2 were characterized by SEM, TEM, XRD, pore size distribution, etc. The results are shown in Figure 3-6 As shown:
[0131] Figure 3 The pore size distribution diagrams of nZVI, SnZVI, AC, SnZVI-AC-1 and SnZVI-AC-2 are shown in Figure 2. Figure 3 It shows that compared with AC, the specific surface area of SnZVI-AC decreased by 810.0-905.3 m 2 / g, the average pore volume decreased by 0.22-0.26cm 3 / g, the pore size increased by 0.53-1.36nm. SnZVI was loaded on the surface and pores of AC, resulting in a decrease in its specific surface area and pore volume, but it also expanded the pore size of AC and generated new pores.
[0132] Figure 4 The TEM images of SnZVI-AC-1, SnZVI and AC are shown in Figure 2. The sulfurization method used in the present invention is a one-step synthesis method, namely, Fe 2+ Reduction of Fe 0 The sulfurization of SnZVI was carried out simultaneously, and the optimal S / Fe ratio was 0.5, which avoided the situation that the SnZVI sulfurization was incomplete due to the low S / Fe ratio and the generated substances were mostly iron-sulfur mixtures due to the high S / Fe ratio. The outer surface of the synthesized SnZVI will be covered with a layer of flocculent sulfide, which will increase its specific surface area and be more conducive to loading on porous materials. 0 and part of S are wrapped inside, greatly retaining Fe 0 AC has a large size, an irregular honeycomb structure, and abundant pores, which provide a large number of sites for the loading of SnZVI. SnZVI-AC forms an iron-carbon loading structure, that is, SnZVI is loaded on the surface and pores of AC, which improves the dispersion of SnZVI while reducing its contact area with the external environment.
[0133] Figure 5 SEM images of SnZVI-AC-1 and SnZVI-AC-2. As the AC loading amount increases, the size of SnZVI loaded on AC becomes smaller. This may be because AC improves the dispersibility of SnZVI and provides more loading sites, resulting in a smaller size of the synthesized SnZVI.
[0134] Figure 6 XRD patterns of SnZVI-AC, SnZVI, nZVI and AC. Fe 0 peak, indicating that Fe0 With good crystallinity, the Fe 0 The peaks are at 44.74°, 65.54° and 82.40°. The Fe 0 The peaks are at 44.44°, 64.74°, and 81.82°, indicating that the sulfurization process of SnZVI does not only occur on its surface, but S also embeds into Fe 0 In the 0 The peak shifts and expands the lattice to form Fe-S alloys. FeS peaks are found on SnZVI and SnZVI-AC, indicating that the iron sulfide of SnZVI is mainly FeS, but due to the low crystallinity of FeS, its peak shape is wide and the peak intensity is weak. 2 O 3 The peak indicates that Fe 0 Oxidation occurred during the preparation and characterization process.
[0135] Test Example 3
[0136] Adsorption kinetics of materials on salmon sperm DNA in water:
[0137] Figure 7 The kinetic model of AC, SnZVI, SnZVI-AC-1, and SnZVI-AC-2 is shown in Figure 2. In the adsorption system, the kinetic model can well describe the adsorption process and adsorption properties. The adsorption amounts of SnZVI-AC-1, SnZVI-AC-2, SnZVI, and AC are 117.2 mg / g, 93.3 mg / g, 58.9 mg / g, and 16.1 mg / g, respectively, which proves that SnZVI loaded with AC can significantly improve the adsorption capacity of DNA. The adsorption of DNA on SnZVI-AC, SnZVI, and AC was fitted using pseudo-first-order kinetics and pseudo-second-order kinetics. 2 Compared with the results of the previous studies, the adsorption of DNA by SnZVI-AC is more suitable to be described by the pseudo-second-order kinetic model, while the pseudo-second-order adsorption kinetic model mainly shows that chemical adsorption plays a key role in the whole adsorption process, which indicates that the adsorption of DNA by SnZVI-AC in heterogeneous systems is mainly based on chemical adsorption.
[0138] Isotherm model of materials for salmon sperm DNA in water:
[0139] Figure 8Table 2 is the isotherm model of AC, SnZVI, SnZVI-AC-1, SnZVI-AC-2, respectively. The adsorption between DNA and SnZVI-AC can be well described by the Freundlich and Langmuir models. The adsorption of DNA by SnZVI-AC is more suitable to be described by the Freundlich model; while the Langmuir model mainly describes the monolayer adsorption of homogeneous systems, the Freundlich model is used to describe the multilayer adsorption of heterogeneous systems, indicating that the adsorption of DNA by SnZVI-AC is mainly multilayer adsorption, which is consistent with the intraparticle diffusion model. The parameter n of the Freundlich model is related to the energy heterogeneity of the system. The 1 / n value < 1 indicates multiphase adsorption. The smaller the 1 / n, the easier it is for the adsorbent to adsorb. The 1 / n value of SnZVI-AC is: SnZVI-AC-1 (2.67 ± 0.30) > SnZVI-AC-2 (2.08 ± 0.12), indicating that SnZVI in SnZVI-AC is the main active substance for adsorbing DNA. SnZVI can continuously provide positive charge for AC, promoting its adsorption of DNA (Table 2). Therefore, the greater the amount of SnZVI loaded on AC, the wider the energy distribution of its adsorption site, which in turn leads to a stronger ability to adsorb DNA.
[0140] Table 2. Langmuir model and Freundlich model fitting parameters of SnZVI-AC-1, SnZVI-AC-2, SnZVI and AC adsorbing salmon sperm DNA
[0141]
[0142] SnZVI-AC is of great significance in removing salmon sperm DNA from aqueous solution, which can be explained from the following aspects:
[0143] ① Improve water quality safety: DNA in water may carry pathogens or harmful genes, threatening the health of humans and ecosystems. Using SnZVI-AC to remove salmon sperm DNA in water can help reduce these potential dangers, improve water quality safety, and protect public health.
[0144] ② High efficiency removal ability: SnZVI-AC has a high specific surface area and strong reducing ability, which makes it excellent in adsorbing and degrading organic pollutants (including DNA). Compared with traditional treatment methods, SnZVI-AC can more effectively remove DNA from water in a shorter time, which has significant technical advantages.
[0145] ③ Sustainable development: The use of carbon-based materials and nano-zero-valent iron composites not only improves the stability and regeneration capacity of the material, but also reduces the processing cost and environmental burden. The application of SnZVI-AC materials is in line with the concept of sustainable development and promotes the development of green environmental protection technology.
[0146] ④ Response to pollution incidents: In environmental emergency response, such as laboratory leaks, it is crucial to quickly and effectively remove DNA from water. SnZVI-AC can respond quickly and provide an efficient means of emergency response.
[0147] ⑤ Expand the application of nanomaterials: Research and application of removing salmon sperm DNA from water not only expands the application of nanomaterials in environmental governance, but also provides a reference and reference for the treatment of other similar pollutants, and promotes the further development of nanotechnology in environmental science.
[0148] The application of SnZVI-AC in removing salmon sperm DNA from aqueous solutions has multiple significances, including improving water safety, efficiently removing pollution, promoting sustainable development, responding to sudden pollution incidents, and expanding the application of nanomaterials. The research and application of this technology not only has important practical value for environmental governance, but also provides broad prospects for the development and application of nanomaterials in the future.
[0149] Test Example 4
[0150] Removal of antibiotic resistance genes in soil:
[0151] Fig. 9 The soil-materials that were cultivated for 25 days were separated and XRD analysis was performed on the materials to observe their phase composition. The main phase of brown soil and red soil is SiO 2 , while the diffraction angles of C and Si are similar. Considering the actual addition, it is believed that the peaks of the original SnZVI-AC and AC are C peaks, while the SnZVI-AC and AC separated from brown soil and red soil are inevitably combined with soil particles, so their performance is mainly Si peaks. By comparing the AC spectra before and after application, it is found that except for the SiO 2 The peak of C covered the peak of C, while the peak intensity of other C peaks decreased but could still be observed, which indicated that AC was not easy to combine with soil and was relatively stable. During the high-temperature carbonization process, the biomass of AC was highly aromatic and had strong stability. Even after the external structure was oxidized, its internal structure could still exist stably in the soil. However, SnZVI-AC and SnZVI only showed Fe 2 O 3 The peak of Fe 0The peaks of Fe0 and FeS can be detected, but can still be separated by a magnet. This may be because the surfaces of SnZVI and SnZVI-AC are coated by soil components, which leads to the fact that the peaks of Fe0 and FeS are not detected.
[0152] Fig.10 As shown, FTIR analysis of the soil and separated materials was performed to determine the interaction and binding of the materials with the soil components. 2930cm -1 It is the absorption peak of soil organic matter (OM); 1440cm -1 It is the absorption peak of carbonate in soil; 1030cm -1 and 795cm -1 It is caused by the symmetrical stretching vibration of Si-O-Si bond; 460cm -1 The peaks near the 20° are mainly caused by the stretching vibration of the Fe-O bond. The composition of brown soil and red soil is complex, mainly composed of silicon dioxide (Si-O-Si), silicate (Si-O), carbonate (CO 3 2- ) and OM, while the separated SnZVI-AC and SnZVI showed Si-O-Si, Si-O and OM peaks, indicating that SnZVI-AC and SnZVI combined with silicates and silica in the soil and attached a small amount of organic matter; the Si-O-Si peak had the highest peak intensity among all samples, because silica is the most difficult primary mineral to weather in the soil, accounting for more than 20% in the soil. OM and silicates in the soil can combine with the iron ions produced by the oxidation and dissolution of SnZVI to form a stable complex, and are deposited on the surface of the material under the action of gravity, which leads to the internal Fe, FeS and Fe 2 O 3 The AC surface contains more hydrophilic functional groups, which will adhere soil particles to its pores and surface, and then gradually age.
[0153] Fig.11 ( Fig.11Different letters in the table indicate significant differences between different groups or conditions. The significant differences were analyzed by one-way ANOVA test using IBM SPSS Statistics 26. The abundance of the three ARGs in the brown soil system was higher than that in the red soil system. Combined with the physical and chemical properties of the soil, brown soil contains higher nitrogen, phosphorus and organic matter, which is more suitable for microbial growth and reproduction. Therefore, SnZVI-AC has a higher removal effect on ARGs in red soil than in brown soil (red soil: 83.60%-94.89%; brown soil: 81.49%-89.07%). Without the addition of SnZVI-AC, SnZVI and AC, the abundance of ARGs in brown soil and red soil did not fluctuate much in the short term (5-25 days), indicating that the microcosm system constructed in this study can maintain a relatively stable state in the short term without the interference of external factors. When the addition of SnZVI-AC, SnZVI and AC is the same, the abundance of the three ARGs in the brown soil and red soil systems does not change significantly over time. With the increase of SnZVI-AC, SnZVI and AC addition, the abundance of ARGs decreased rapidly. After adding 5% SnZVI-AC and culturing for 5 days, the abundance of sul1, tetA and ermF in brown soil decreased by 61.52%, 86.28% and 79.46%, and the abundance of sul1, tetA and ermF in red soil decreased by 81.60%, 70.45% and 94.87%. The removal of ARGs in soil by SnZVI-AC, SnZVI and AC basically reached saturation within 5 days. After 15 and 25 days, ARGs slowly decreased, among which the growth of SnZVI was the slowest (ARGs removal rate changed <1%). Combined with the characterization analysis in 4.3.2, it is speculated that the addition of SnZVI, SnZVI-AC and AC in the short term will adsorb ARGs in the soil and change the original physical and chemical properties of the soil, which may lead to changes in the microbial community structure, thereby reducing the abundance of ARGs. However, as the application time increases, the material gradually ages, resulting in a decrease in its adsorption performance, while the soil also gradually stabilizes its physical and chemical properties through biological / abiotic means, resulting in a slow decrease in the abundance of ARGs.
[0154] SnZVI-AC is of great significance in removing antibiotic resistance genes (ARGs) in soil, which can be explained from the following aspects:
[0155] ① Environmental risks of antibiotic resistance genes: Antibiotic resistance genes (ARGs) can spread between microorganisms, causing antibiotic treatment failure and posing a threat to public health. ARGs enter the soil environment through wastewater, livestock and poultry waste, etc., causing soil ecosystem pollution. ARGs are persistent in the environment and difficult to degrade naturally, requiring effective means to remove.
[0156] ② Combined with the characteristics of SnZVI-AC, due to its unique physical and chemical properties, it can effectively remove ARGs in the soil. Its application can increase soil pH and dissolved organic carbon content and improve the soil environment.
[0157] ③ Mechanism of removing ARGs: SnZVI-AC directly adsorbs ARGs through surface complexation, reducing their activity and mobility in the soil. It can also indirectly fix ARGs associated with heavy metals by promoting the formation of metal sulfide precipitation. It can also promote the growth of bacteria, which can further promote the degradation and transformation of ARGs.
[0158] ④ Improve soil nutrients and microbial diversity: Increase effective nutrients. SnZVI-AC increases the content of ammonium nitrogen and available potassium in the soil, which is conducive to plant growth. Improve microbial communities, which promotes the increase of soil microbial community functional abundance and enhances the self-repair ability of the soil.
[0159] ⑤ Reduce the risk of spreading antibiotic resistance genes: SnZVI-AC fixes ARGs, reducing the risk of their horizontal gene transfer through mobile gene elements (MGEs), which can also inhibit the growth of drug-resistant bacteria: the improved soil environment is not conducive to the growth of drug-resistant bacteria, thereby reducing the spread of ARGs.
[0160] ⑥ Environmentally friendly and sustainable: Compared with other heavy metal remediation materials, SnZVI-AC has lower ecotoxicity. The addition of activated carbon improves the sustainability of the material and promotes the recycling of resources.
[0161] Finally, it should be noted that the above content is only used to illustrate the technical solution of the present invention, rather than to limit the scope of protection of the present invention. Simple modifications or equivalent substitutions of the technical solution of the present invention by ordinary technicians in this field do not deviate from the essence and scope of the technical solution of the present invention.
Claims
1. A method for preparing carbon-supported sulfided nano zero-valent iron, characterized in that: The following steps are involved: S1: NaBH4 and Na2S2O4 are mixed with a solvent to obtain a mixed solution 1; the concentration of NaBH4 in the mixed solution is 0.25-0.29 mol / L, and the concentration of Na2S2O4 in the mixed solution is 0.03-0.034 mol / L; S2: Activated carbon is mixed with FeSO4·7H2O solution, mixed solution 1 is added, stirred to sulfide, washed, and dried to obtain carbon-based sulfide nano zero-valent iron; The molar ratio of S in the Na2S2O4 to Fe in the FeSO4·7H2O is 0.4-0.6:1; The mass ratio of iron in the FeSO4·7H2O to activated carbon is 1:1-3.
2. The preparation method according to claim 1, characterized in that: The concentration of NaBH4 in the mixed solution described in S1 is 0.26-0.28 mol / L.
3. The preparation method according to claim 1, characterized in that: The concentration of Na2S2O4 in the mixed solution described in S1 is 0.03-0.035 mol / L.
4. The preparation method according to claim 1, characterized in that: The stirring time in S2 is 1-1.5h, and the stirring speed is 700-900r / min.
5. The preparation method according to claim 1, characterized in that: The molar ratio of S in the Na2S2O4 to Fe in the FeSO4·7H2O is 0.5:
1.
6. The preparation method according to claim 1, characterized in that: The mass ratio of iron in the FeSO4·7H2O to activated carbon is 1:1 or 1:
3.
7. The preparation method according to claim 1, characterized in that: The cleaning described in S2 is to use ethanol and water to clean the precipitate obtained by sulfidation; the volume ratio of the ethanol to water is 1:0.9-1.
1.
8. The preparation method according to claim 1, characterized in that: The specific operation of freeze drying described in S2 is: drying under vacuum conditions of -52°C-60°C for 10-12h.
9. Use of the carbon-supported sulfide nano-zero-valent iron according to any one of claims 1 to 8 in treating genetic pollutants in soil.
10. The use according to claim 9, characterized in that: The soil is selected from at least one of brown soil or red soil.