Preparation method and application of In2O3 / W18O49 heterojunction nanofiber photocatalyst
Through the preparation of In2O3/W18O49 heterojunction nanofiber photocatalyst, the problem of low photocatalyst efficiency is solved, and a solution that improves photocatalytic activity and hydrogen evolution performance is achieved, which is suitable for large-scale production.
Patent Information
- Application Number
- CN202411112911.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-08-14
AI Technical Summary
The existing photocatalysts have low efficiency in using solar energy to decompose water to produce hydrogen by using solar energy, which is difficult to meet energy needs, and the solar energy utilization rate of In2O3 is low and the carrier complexity rate is high.
The preparation method of In2O3/W18O49 heterojunction nanofiber photocatalyst is prepared by electrospinning and solvent thermal method to prepare ultra-long one-dimensional structure In2O3/W18O49 heterojunction nanofibers with ultra-long one-dimensional structure to form heterojunctions to improve photogenerating electron holes Separation efficiency and photocatalysts are obtained by hydrothermal reaction and drying.
It improves the separation efficiency and photocatalytic activity of carriers, enhances visible photocatalytic activity and photocatalytic hydrogen evolution performance, and the preparation method is simple, environmentally friendly, low-cost, and is suitable for large-scale production.
Smart Images

Figure CN118874457A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of photocatalytic materials and specifically relates to an In2O3 / W 18 O 49 Preparation method and application of heterojunction nanofiber photocatalyst. Background Art
[0002] Due to the continuous growth of global energy consumption and the increasingly serious environmental pollution problem, it has become a top priority to find clean and sustainable energy to replace traditional fossil fuels. As an inexhaustible and widely distributed clean energy, solar energy has great potential. In order to develop clean and sustainable renewable energy, the use of solar energy to photocatalytically decompose water to produce hydrogen has become a research hotspot. Photocatalytic decomposition of water to produce hydrogen is considered to be one of the most promising technologies for developing clean and sustainable hydrogen energy due to its advantages of low cost, energy saving and environmental protection. However, the efficiency of current photocatalysts to produce hydrogen by photocatalytically decomposing water using solar energy is relatively low, which is difficult to meet human demand for energy.
[0003] In2O3 is widely used in the field of photocatalytic water decomposition and hydrogen production due to its excellent conductivity, stability, wide bandgap and small resistivity. However, pure In2O3 faces the problems of low solar energy utilization and high carrier complexation rate. Therefore, synthetic heterojunction is an effective method to improve the solar energy utilization of In2O3 and reduce the recombination of electron-hole pairs. 18 O 49 The formation of heterojunction can improve the separation efficiency of photogenerated electrons and holes, thereby improving the photocatalytic activity; and In2O3 / W 18 O 49 There has been no report on heterojunction nanofibers as photocatalysts for hydrogen evolution. Summary of the invention
[0004] In order to solve the above problems, the present invention provides an In2O3 / W 18 O 49 Preparation method and application of heterojunction nanofiber photocatalyst.
[0005] The technical solution adopted by the present invention is:
[0006] In2O3 / W 18 O 49 The preparation method of heterojunction nanofiber photocatalyst comprises the following steps:
[0007] 1) dissolving indium nitrate tetrahydrate in a mixed solution of N,N-dimethylformamide and ethanol until completely dissolved, adding polyvinyl pyrrolidone powder to the mixed solution, stirring until the solution is colorless and transparent, and performing electrospinning at a voltage of 15 kV and a distance of 12 cm from a collecting plate to collect nanofibers;
[0008] 2) The collected nanofibers are torn with scissors and tweezers and placed in a porcelain boat, which is then placed in a low-temperature muffle furnace for calcination to obtain In2O3 nanofibers;
[0009] 3) Dissolve tungsten hexachloride in anhydrous ethanol, stir the solution until it turns blue, place the In2O3 nanofibers obtained in step 2) in an autoclave filled with tungsten hexachloride solution for hydrothermal reaction, wash the sample after the reaction, and dry it to obtain In2O3 / W 18 O 49 Heterojunction nanofiber photocatalysts.
[0010] Furthermore, in the above preparation method, in step 1), the amount of indium nitrate tetrahydrate is 0.8 g, the amount of polyvinyl pyrrolidone powder is 1 g, the amount of NN-dimethylformamide is 4 mL, and the amount of ethanol is 6 mL.
[0011] Furthermore, in the above-mentioned preparation method, in steps 1) and 3), the stirring method is to use a magnetic stirrer for stirring.
[0012] Furthermore, in the above preparation method, step 2), the calcination temperature is 550° C., the heating rate is 1° C. / min, and the calcination time is 2 h.
[0013] Furthermore, in the above preparation method, in step 3), the mass ratio of tungsten hexachloride to In2O3 nanofibers is 5%, 25% or 35%.
[0014] Furthermore, in the above preparation method, in step 3), the temperature of the hydrothermal reaction is 160° C. and the reaction time is 6 hours.
[0015] Furthermore, in the above preparation method, in step 3), the drying temperature is 40° C. and the drying time is 2 h.
[0016] In2O3 / W prepared by any of the above preparation methods 18 O 49 Application of heterojunction nanofiber photocatalysts in photocatalytic water decomposition for hydrogen evolution.
[0017] Further, the above application method is as follows: take In2O3 / W 18 O 49The heterojunction nanofiber photocatalyst is uniformly dispersed in a mixed solution of deionized water, triethanolamine and chloroplatinic acid, and argon gas is continuously introduced into the container containing the mixed solution at a constant flow rate to obtain a relatively vacuum environment, and water is photocatalytically decomposed to release hydrogen under visible light irradiation conditions.
[0018] Furthermore, for the above applications, according to the solid-liquid ratio, In2O3 / W 18 O 49 Heterojunction nanofiber photocatalyst: deionized water: triethanolamine: chloroplatinic acid = 20 mg: 18 mL: 2 mL: 15 μL.
[0019] The beneficial effects of the present invention are:
[0020] 1. The present invention uses electrospinning and solvent thermal methods to prepare In2O3 / W 18 O 49 Heterojunction nanofiber photocatalysts have an ultra-long one-dimensional structure, which can improve the carrier separation efficiency and enhance the photocatalytic activity.
[0021] 2. In2O3 / W prepared by the present invention 18 O 49 Heterojunction nanofiber photocatalysts have a stronger ability to absorb visible light and are an effective way to improve visible light catalytic activity.
[0022] 3. In2O3 / W prepared by the present invention 18 O 49 Heterojunction nanofiber photocatalysts have good photocatalytic hydrogen evolution performance, and the method is simple to prepare, environmentally friendly, non-toxic, low-cost, and conducive to large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 In2O3, W 18 O 49 、In2O3 / W 18 O 49 X-ray diffraction pattern of heterojunction nanofiber photocatalyst.
[0024] Figure 2 In2O3, W 18 O 49 、In2O3 / W 18 O 49 The hydrogen production-time curve of water decomposition by heterojunction nanofiber photocatalyst. DETAILED DESCRIPTION
[0025] Example 1
[0026] In2O3 / W 18 O 49The preparation method of heterojunction nanofiber photocatalyst is as follows:
[0027] Dissolve 0.8g of indium nitrate tetrahydrate in a mixed solution of 4mL N,N-dimethylformamide (DMF) and 6mL ethanol and stir magnetically until completely dissolved. Add 1g of polyvinyl pyrrolidone powder (PVP) and stir until colorless and transparent. Draw the obtained solution into a plastic syringe for electrospinning. The applied voltage is 15KV, the distance between the needle tip and the collector is 12cm, and a dense nanofiber is collected on aluminum foil with tweezers. Cut the dense nanofiber into 5cm×8cm rectangular slices with scissors and put them into a porcelain boat, and then put them into a muffle furnace and calcine at 550℃ for 2h (heating rate is 1℃ / min) to obtain In2O3 nanofibers. 7 mg of WCl6 was added and dissolved in 12 mL of anhydrous ethanol. The solution was stirred magnetically until it turned blue. Then 20 mg of In2O3 nanofibers were added and placed in a hydrothermal reactor for hydrothermal reaction at 160 °C for 6 h. After cooling naturally to room temperature, the nanofibers were washed three times with deionized water and anhydrous ethanol respectively and dried at 40 °C for 2 h to obtain In2O3 / W 18 O 49 Heterojunction nanofiber photocatalysts.
[0028] Figure 1 In2O3 / W prepared in Example 1 18 O 49 X-ray diffraction pattern of heterojunction nanofiber photocatalyst. Characteristic diffraction peaks appear at 2θ=21.6°, 30.8°, 35.5°, 51.0° and 60.9°, corresponding to (211), (222), (400), (440) and (622) crystal planes, which is consistent with the In2O3 PDF standard card (PDF#88-2160). Characteristic diffraction peaks appear at 2θ=23.28° and 48.02°, corresponding to (010) and (020) crystal planes, which is consistent with the W 18 O 49 The PDF standard card (PDF#71-2450) is consistent. When the two are combined, Figure 1 It can be seen that the peaks of both substances appear in the composite sample In2O3 / W 18 O 49 , indicating that the two substances successfully combined.
[0029] Example 2
[0030] At room temperature and pressure, take 20 mg of In2O3 / W prepared in Example 1 18 O 49The heterojunction nanofiber photocatalyst was uniformly dispersed in a mixed solution of 18 mL of deionized water, 2 ml of TEOA (triethanolamine) and 15 μL of chloroplatinic acid. Argon gas was continuously introduced into the container containing the mixed solution at a constant flow rate (40 mL / min) to obtain a relative vacuum environment. The container was then irradiated with a xenon lamp. After every 30 minutes of illumination reaction, the upper gas was extracted from the container with a syringe, and the hydrogen concentration in the upper gas was tested with a gas chromatograph.
[0031] Figure 2 The photocatalytic decomposition of water produces hydrogen over time. It can be seen that after 30 minutes of light reaction, In2O3 / W 18 O 49 The hydrogen production is 177.7 μmol / g, which is 14.3 times that of pure In2O3 and 1.3 times that of pure W 18 O 49 3.8 times the hydrogen production.
Claims
1. In2O3 / W 18 O 49 The method for preparing heterojunction nanofiber photocatalyst is characterized in that: The steps include: 1) dissolving indium nitrate tetrahydrate in a mixed solution of N,N-dimethylformamide and ethanol until completely dissolved, adding polyvinyl pyrrolidone powder to the mixed solution, stirring until the solution is colorless and transparent, and performing electrospinning at a voltage of 15 kV and a distance of 12 cm from a collecting plate to collect nanofibers; 2) The collected nanofibers are torn with scissors and tweezers and placed in a porcelain boat, which is then placed in a low-temperature muffle furnace for calcination to obtain In2O3 nanofibers; 3) Dissolve tungsten hexachloride in anhydrous ethanol, stir the solution until it turns blue, place the In2O3 nanofibers obtained in step 2) in an autoclave filled with tungsten hexachloride solution for hydrothermal reaction, wash the sample after the reaction, and dry it to obtain In2O3 / W 18 O 49 Heterojunction nanofiber photocatalysts.
2. The preparation method according to claim 1, characterized in that: In step 1), the amount of indium nitrate tetrahydrate is 0.8 g, the amount of polyvinyl pyrrolidone powder is 1 g, the amount of NN-dimethylformamide is 4 mL, and the amount of ethanol is 6 mL.
3. The preparation method according to claim 1, characterized in that: In steps 1) and 3), the stirring method is to use a magnetic stirrer for stirring.
4. The preparation method according to claim 1, characterized in that: Step 2), the calcination temperature is 550°C, the heating rate is 1°C / min, and the calcination time is 2h.
5. The preparation method according to claim 1, characterized in that: In step 3), the mass ratio of tungsten hexachloride to In2O3 nanofibers is 5%, 25% or 35%.
6. The preparation method according to claim 1, characterized in that: In step 3), the temperature of the hydrothermal reaction is 160° C. and the reaction time is 6 h.
7. The preparation method according to claim 1, characterized in that: In step 3), the drying temperature is 40° C. and the drying time is 2 h.
8. In2O3 / W prepared by the preparation method according to any one of claims 1 to 7 18 O 49 Application of heterojunction nanofiber photocatalysts in photocatalytic water decomposition for hydrogen evolution.
9. The use according to claim 8, characterized in that: The method is as follows: Take In2O3 / W 18 O 49 The heterojunction nanofiber photocatalyst is uniformly dispersed in a mixed solution of deionized water, triethanolamine and chloroplatinic acid, and argon gas is continuously introduced into the container containing the mixed solution at a constant flow rate to obtain a relatively vacuum environment, and water is photocatalytically decomposed to release hydrogen under visible light irradiation conditions.
10. The use according to claim 9, characterized in that: According to the solid-liquid ratio, In2O3 / W 18 O 49 Heterojunction nanofiber photocatalyst: deionized water: triethanolamine: chloroplatinic acid = 20 mg: 18 mL: 2 mL: 15 μL.
Citation Information
Patent Citations
Pt / In2O3-x composite nanofiber material as well as preparation method and application thereof
CN114703659A
W18O49 / C / g-C3N4 heterojunction nanofiber photocatalyst as well as preparation method and application thereof
CN116020514A
Nb2O5 / W18O49 heterojunction nanofiber photocatalyst as well as preparation method and application thereof
CN118105970A
Photocatalyst carrier, and producing method thereof
JP2002028494A