Application of difunctional material for coupling carbon dioxide capture with methane dry reforming in oxygen-containing flue gas treatment
By using copper-modified nickel/calcium oxide composite materials, the problems of catalytic component passivation and carbon deposition in the ICCU-DRM process of oxygen-containing flue gas were solved, achieving efficient CO2 and CH4 conversion, improving the stability and anti-carbon deposition performance of the materials, and broadening the application range.
Patent Information
- Application Number
- CN202410899267.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-07-05
AI Technical Summary
In oxygen-containing flue gas, existing carbon dioxide capture coupled with methane dry reforming technology suffers from catalytic component passivation and carbon deposition caused by oxygen, resulting in decreased CO2 conversion rate and hindered capture performance, making it difficult to achieve an efficient ICCU-DRM process.
A copper-modified nickel/calcium oxide composite material is used. The excellent reduction properties of copper promote the reduction of NiO to metallic nickel, suppressing in-situ delay phenomenon and carbon deposition. At the same time, zirconium oxide is added to improve the stability of the material, forming a copper and zirconium oxide modified nickel/calcium oxide composite material.
It significantly improves the conversion rate of CO2 and CH4, reduces the H2/CO ratio, and inhibits carbon deposition. The material exhibits good cycle stability and resistance to coke deposition at high temperatures, thus broadening the application possibilities of ICCU-DRM in oxygen-containing flue gas.
Smart Images

Figure CN118874473A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of oxygen-containing flue gas treatment, and in particular to the application of a dual-functional material for carbon dioxide capture coupled with methane dry reforming in oxygen-containing flue gas treatment. Background Art
[0002] Recently, with the increasing emission of carbon dioxide (CO2) year by year, environmental problems have become more and more serious. In order to reduce CO2 emissions and achieve the "dual carbon" goal, integrated CO2 capture and utilization (ICCU) technology has emerged. ICCU technology couples CO2 capture technology and CO2 conversion technology to achieve CO2 capture and in-situ conversion in the same temperature and reactor, which can greatly reduce industrial energy consumption and has good application prospects. Generally, CO2 adsorbents are divided into high-temperature (>400℃), medium-temperature (200~400℃) and low-temperature (<200℃) adsorbents according to the different CO2 capture temperatures. In the conversion stage, it is usually coupled with dry reforming of methane (DRM), reverse water gas and methanation reactions (Equations 1~3). Among them, DRM can convert two greenhouse gases CO2 and CH4 into usable synthesis gas (H2 and CO). When DRM is effectively combined with CO2 capture, the energy consumption of CO2 utilization and the fuel demand for producing synthesis gas are lower than traditional DRM. Therefore, integrated CO2 capture and utilization coupled methane dry reforming (ICCU-DRM) technology is a CO2 emission reduction technology with great application prospects.
[0003] CO2+CH4→2CO+2H2, ΔH 298K = +247 kJ·mol -1 (1)
[0004] CO2+H2→CO+H2O, ΔH 298K = +41.2 kJ·mol -1 (2)
[0005] CO2+4H2→CH4+2H2O, ΔH 298K =-165 kJ·mol -1 (3)
[0006] For ICCU-DRM technology, it is necessary to develop dual-functional materials (DFMs) with both adsorption sites and catalytic sites to achieve fast and stable CO2 capture and conversion efficiency. CaO is widely present in nature and has the characteristics of low cost and high theoretical CO2 absorption capacity. It is usually used as an adsorption material; Ni is considered to be an efficient metal element for converting CO2 and CH4, two bond-stabilized compounds, due to its low cost and high catalytic activity. It is used together with CaO to realize CO2 capture coupled with methane dry reforming (CaLDRM). By switching the atmosphere in one reactor, the CO2 capture and conversion stages can be carried out continuously. The consumption of CO2 in the reaction process reduces the partial pressure of CO2 in the reactor, promotes the calcination of CaCO3, and can reduce the temperature required for the calcination reaction to a certain extent, thereby reducing the deactivation of CaO caused by sintering.
[0007] However, the in-situ delay of DRM caused by the passivation of catalytic components by O2 in actual flue gas cannot be ignored. Due to the presence of O2 in the carbon source, the active component Ni will be oxidized to NiO with almost no catalytic activity. When the in-situ DRM process begins, CH4 reduces NiO to Ni, resulting in a pre-reduction stage that delays CO2 conversion, further leading to a decrease in CO2 conversion rate. CO2 capture performance will also be hindered due to the adverse effects of O2 on the CaO structure.
[0008] Therefore, how to avoid the impact of DRM delay and efficiently realize ICCU-DRM under the condition of oxygen content in flue gas is an issue worthy of attention. Summary of the invention
[0009] The present invention provides an application of a dual-functional material for carbon dioxide capture coupled with methane dry reforming in oxygen-containing flue gas treatment. The present invention utilizes copper to modify a nickel / calcium oxide composite material, and on the basis of retaining the dual-functional characteristics of the adsorption site and catalytic site of the nickel / calcium oxide composite material, copper is used to reduce nickel oxide to metal elemental nickel, so that the activity of the nickel / calcium oxide composite material in oxygen-containing flue gas will not decrease, and the DRM phenomenon and the generation of inactivating substances, namely carbon deposition, in the ICCU-DRM process are significantly suppressed, thereby ensuring the efficient ICCU-DRM of the nickel / calcium oxide composite material in oxygen-containing flue gas.
[0010] In order to achieve the above object, the present invention provides the following technical solutions:
[0011] The present invention provides an application of a dual-functional material for carbon dioxide capture coupled with methane dry reforming in oxygen-containing flue gas treatment. The dual-functional material is a copper-modified nickel / calcium oxide composite material. The dual-functional material can inhibit in-situ delay phenomenon and carbon deposition.
[0012] All nickel / calcium oxide composite materials in the present application are actually composite materials of nickel oxide and calcium oxide, which are often referred to as nickel / calcium oxide composite materials in the art.
[0013] The present application utilizes the excellent reduction performance of Cu. Furthermore, Cu can promote the activation of CH4 and produce active hydrogen (H*), further promoting the reduction of NiO to metal element Ni to quickly exert catalytic effect, so that the in-situ delay of the DRM stage is suppressed. At the same time, the CH4 conversion rate can be greatly improved, and it has a significant effect on reducing the H2 / CO ratio. The lower H2 / CO ratio indicates that carbon deposition is effectively suppressed.
[0014] The present application provides a new application idea for copper-modified nickel / calcium oxide composite materials and solves the problem of realizing high-efficiency ICCU-DRM under oxygen-containing flue gas.
[0015] Preferably, in the treatment of oxygen-containing flue gas, the bifunctional material has a carbon dioxide conversion rate of 92-97%, a methane conversion rate of 42-57%, and a H2 / CO ratio of 2.35-2.36 at a temperature of 600°C.
[0016] Preferably, the preparation method of the dual-functional material comprises: dissolving copper salt, nickel salt and calcium salt in water, adding anhydrous citric acid, stirring until the solution turns into a gel state, drying and calcining to obtain a copper-modified nickel / calcium oxide composite material.
[0017] Preferably, the dual-functional material is a nickel / calcium oxide composite material modified by copper and zirconium oxide, and the dual-functional material can suppress in-situ delay phenomenon and carbon deposition.
[0018] The present application utilizes the excellent reduction performance of Cu. Furthermore, Cu can promote the activation of CH4 and produce active hydrogen (H*), further promoting the reduction of NiO to metallic element Ni to quickly exert a catalytic effect, so that the in-situ delay of the DRM stage is suppressed. At the same time, the CH4 conversion rate can be greatly improved, and it has a significant effect on reducing the H2 / CO ratio. The lower H2 / CO ratio indicates that carbon deposition can be effectively suppressed. ZrO2 is used as a stabilizer because of its high Tamman temperature to improve the cycle performance of CaO and thus improve the overall cycle stability of the dual-functional material.
[0019] Modification of nickel / calcium oxide composite materials by utilizing the strong reducing properties of Cu and the high stability of ZrO2 can effectively inhibit the in-situ DRM delay caused by oxygen-containing flue gas and improve the CaLDRM performance, thereby achieving a significant increase in CH4 conversion rate and recycling under actual flue gas conditions, making its application in actual industry possible.
[0020] In summary, the present application provides a new application idea for nickel / calcium oxide composite materials modified by copper and zirconium oxide, and solves the problem of realizing high-efficiency ICCU-DRM under oxygen-containing flue gas.
[0021] Preferably, in the treatment of oxygen-containing flue gas, the bifunctional material has the following conditions: at a temperature of 600°C, the conversion rate of carbon dioxide is 98-99%, the conversion rate of methane is 44-55%, and the H2 / CO ratio is 2.00-2.12; after five cycles at a temperature of 650°C, the conversion rate of methane is 66.44%.
[0022] Preferably, the preparation method of the dual-functional material comprises: dissolving copper salt, zirconium salt, nickel salt and calcium salt in water, adding anhydrous citric acid, stirring until the solution turns into a gel state, drying and calcining to obtain a copper and zirconium oxide modified nickel / calcium oxide composite material.
[0023] Preferably, the copper salt, zirconium salt, nickel salt and calcium salt are copper nitrate, zirconium nitrate, nickel nitrate and calcium nitrate respectively.
[0024] Preferably, the molar ratio of the nickel salt to the copper salt is (1-9):1.
[0025] More preferably, the molar ratio of the nickel salt to the copper salt is (2-9):1.
[0026] More preferably, the molar ratio of the nickel salt to the copper salt is (5-9):1.
[0027] Further preferably, the molar ratio of the nickel salt to the copper salt is 9:1.
[0028] Preferably, the sum of the molar amounts of the copper salt, zirconium salt, nickel salt and calcium salt is a mol, the molar amount of the anhydrous citric acid is a mol, and the molar amount of the water is 30a to 45a mol.
[0029] Here, a can be any value greater than zero. The applicant would like to emphasize the proportional relationship between the sum of the molar amounts of copper salt, zirconium salt, nickel salt, and calcium salt, the molar amount of anhydrous citric acid, and the molar amount of water.
[0030] Preferably, the stirring temperature is 85-100°C.
[0031] More preferably, the stirring temperature is 90°C.
[0032] Preferably, the drying temperature is 120-140° C., and the drying time is 8-24 hours.
[0033] More preferably, the drying temperature is 130° C., and the drying time is 12 h.
[0034] Preferably, the calcination temperature is 650-750° C., the calcination time is 3-5 hours, and the calcination heating rate is 4-6° C. / min.
[0035] Further preferably, the calcination temperature is 700° C., the calcination time is 4 h, and the calcination heating rate is 5° C. / min.
[0036] Therefore, the present invention has the following beneficial effects:
[0037] (1) The present invention utilizes a copper-modified nickel / calcium oxide composite material to obtain a dual-functional material, and provides the possibility of applying the dual-functional material in an efficient ICCU-DRM under oxygen-containing flue gas.
[0038] (2) The present invention utilizes a nickel / calcium oxide composite material modified by copper and zirconium oxide to obtain a dual-functional material, which effectively suppresses the delay phenomenon in the conversion stage after capturing oxygen-containing flue gas, and the CH4 conversion rate is increased by more than 10%; it has good cycle stability at high temperatures, and still has stable and considerable conversion performance after 5 cycles at a temperature of 650°C; and it has better anti-carbon deposition performance than the nickel / calcium oxide composite material under the same conditions.
[0039] (3) The present invention provides a method of using a copper-modified nickel / calcium oxide composite material to inhibit the DRM phenomenon and resist carbon deposition, thereby broadening the path to achieving high-efficiency ICCU-DRM under oxygen-containing flue gas.
[0040] (4) The present invention provides a nickel / calcium oxide composite material modified by copper and zirconium oxide, which can suppress the DRM phenomenon and resist carbon deposition while realizing the recycling of dual-functional materials, greatly reducing the cost of using dual-functional materials and facilitating industrial applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 Transmission electron microscope images of Ni9Cu1-CaZr before and after the reaction, where a is before the reaction and b is after the reaction;
[0042] Figure 2 It is a real-time curve chart of the change of gas concentration during the performance test of the dual-functional material;
[0043] Figure 3 It is a real-time curve chart of gas concentration changes during the performance test of dual-functional materials at different temperatures. DETAILED DESCRIPTION
[0044] The present invention is further described below in conjunction with specific embodiments. Those of ordinary skill in the art will be able to implement the present invention based on these descriptions. In addition, the embodiments of the present invention involved in the following description are generally only embodiments of a part of the present invention, rather than all embodiments. Therefore, based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work should fall within the scope of protection of the present invention.
[0045] [Example]
[0046] Example 1
[0047] 1. Preparation of bifunctional materials: Dissolve 1.0469g nickel nitrate (Ni(NO3)2·6H2O), 0.0966g copper nitrate (Cu(NO3)2·3H2O), 8.5014g calcium nitrate (Ca(NO3)2·4H2O) and 1.7178g zirconium nitrate (Zr(NO3)4·5H2O) in 31.68mL deionized water and stir evenly. Add 8.4537g anhydrous citric acid to the mixed solution and stir at room temperature for 1h. Place the solution in a 90℃ oil bath and stir vigorously until it reaches a gel state, then dry it at 130℃ overnight. Then, place the dried solid in a muffle furnace and calcine at 700℃ for 4h with a heating rate of 5℃ / min. The obtained bifunctional material is named Ni9Cu1-CaZr. In this embodiment, Ni 2+ :Cu 2+ The molar ratio is 9:1.
[0048] 2. Simulation of CO2 capture coupled with methane dry reforming in oxygen-containing flue gas
[0049] (1) Heating stage: N2 condition, from room temperature to 600 °C, heating rate 5 °C / min;
[0050] (2) Pre-reduction stage: 10% H2, N2 as balance gas, reaction time 120 min;
[0051] (3) N2 purge for 5 min;
[0052] (4) CO2 capture stage: 10% CO2, 6.7% O2, N2 as balance gas, reaction time 60 min;
[0053] (5) N2 purge for 5 min;
[0054] (6) Methane dry reforming stage: 2.5% CH4, reaction time 180 min;
[0055] (7) N2 purge for 5 min.
[0056] The reaction temperature of the whole process was 600°C and the total flow rate was 100 mL / min.
[0057] Example 2
[0058] This embodiment is basically the same as embodiment 1, the difference being that: Ni 2+ :Cu 2+ The molar ratio is 7:3, and the added amount is: 0.8142g nickel nitrate (Ni(NO3)2·6H2O), 0.2899g copper nitrate (Cu(NO3)2·3H2O). The obtained bifunctional material is named Ni7Cu3-CaZr.
[0059] Example 3
[0060] This embodiment is basically the same as embodiment 1, the difference being that: Ni 2+ :Cu 2+ The molar ratio is 5:5, and the added amount is: 0.5816g nickel nitrate (Ni(NO3)2·6H2O), 0.4832g copper nitrate (Cu(NO3)2·3H2O). The obtained bifunctional material is named Ni5Cu5-CaZr.
[0061] Example 4
[0062] 1. Preparation of bifunctional materials: Dissolve 1.0469g of nickel nitrate (Ni(NO3)2·6H2O), 0.0966g of copper nitrate (Cu(NO3)2·3H2O) and 8.5014g of calcium nitrate (Ca(NO3)2·4H2O) in 28.8mL of deionized water and stir evenly. Add 7.6852g of anhydrous citric acid to the mixed solution and stir at room temperature for 1h. Place the solution in a 90°C oil bath and stir vigorously until it reaches a gel state, then dry it at 130°C overnight. Then, place the dried solid in a muffle furnace and calcine at 700°C for 4h with a heating rate of 5°C / min. The obtained bifunctional material is named Ni9Cu1-Ca. In this embodiment, Ni 2+ :Cu 2+ The molar ratio is 9:1.
[0063] 2. Simulation of CO2 capture coupled with methane dry reforming in flue gas containing oxygen
[0064] (1) Heating stage: N2 condition, from room temperature to 600 °C, heating rate 5 °C / min;
[0065] (2) Pre-reduction stage: 10% H2, N2 as balance gas, reaction time 120 min;
[0066] (3) N2 purge for 5 min;
[0067] (4) CO2 capture stage: 10% CO2, 6.7% O2, N2 as balance gas, reaction time 60 min;
[0068] (5) N2 purge for 5 min;
[0069] (6) Methane dry reforming stage: 2.5% CH4, reaction time 180 min;
[0070] (7) N2 purge for 5 min.
[0071] The reaction temperature of the whole process was 600°C and the total flow rate was 100 mL / min.
[0072] Comparative Example 1
[0073] 1. Preparation of bifunctional materials: Dissolve 1.1632g of nickel nitrate (Ni(NO3)2·6H2O), 8.5014g of calcium nitrate (Ca(NO3)2·4H2O) and 1.7178g of zirconium nitrate (Zr(NO3)4·5H2O) in 31.68mL of deionized water and stir evenly. Add 8.4537g of anhydrous citric acid to the mixed solution and stir at room temperature for 1h. Place the solution in a 90℃ oil bath and stir vigorously until it is in a gel state, then dry it at 130℃ overnight. Then, place the dried solid in a muffle furnace and calcine at 700℃ for 4h with a heating rate of 5℃ / min. The obtained bifunctional material is named Ni-CaZr.
[0074] 2. Simulation of CO2 capture coupled with methane dry reforming in flue gas containing oxygen
[0075] (1) Heating stage: N2 condition, from room temperature to 600 °C, heating rate 5 °C / min;
[0076] (2) Pre-reduction stage: 10% H2, N2 as balance gas, reaction time 120 min;
[0077] (3) N2 purge for 5 min;
[0078] (4) CO2 capture stage: 10% CO2, 6.7% O2, N2 as balance gas, reaction time 60 min;
[0079] (5) N2 purge for 5 min;
[0080] (6) Methane dry reforming stage: 2.5% CH4, reaction time 180 min;
[0081] (7) N2 purge for 5 min.
[0082] The reaction temperature of the whole process was 600°C and the total flow rate was 100 mL / min.
[0083] Comparative Example 2
[0084] 1. Preparation of bifunctional materials: Dissolve 1.1632g of nickel nitrate (Ni(NO3)2·6H2O) and 8.5014g of calcium nitrate (Ca(NO3)2·4H2O) in 28.8mL of deionized water and stir evenly. Add 7.6852g of anhydrous citric acid to the mixed solution and stir at room temperature for 1h. Place the solution in a 90℃ oil bath and stir vigorously until it gels, then dry it at 130℃ overnight. Then, place the dried solid in a muffle furnace and calcine at 700℃ for 4h with a heating rate of 5℃ / min. The obtained bifunctional material is named Ni-Ca.
[0085] 2. Simulation of CO2 capture coupled with methane dry reforming in oxygen-containing flue gas
[0086] (1) Heating stage: N2 condition, from room temperature to 600 °C, heating rate 5 °C / min;
[0087] (2) Pre-reduction stage: 10% H2, N2 as balance gas, reaction time 120 min;
[0088] (3) N2 purge for 5 min;
[0089] (4) CO2 capture stage: 10% CO2, 6.7% O2, N2 as balance gas, reaction time 60 min;
[0090] (5) N2 purge for 5 min;
[0091] (6) Methane dry reforming stage: 2.5% CH4, reaction time 180 min;
[0092] (7) N2 purge for 5 min.
[0093] The reaction temperature of the whole process was 600°C and the total flow rate was 100 mL / min.
[0094]
Performance test
[0095] 1. TEM test
[0096] The Ni9Cu1-CaZr dual-functional material obtained in Example 1 was subjected to TEM test, and the results are as follows: Figure 1 Observation Figure 1 It can be seen that the morphology of the nickel / calcium oxide composite material modified by Cu and ZrO2 did not change significantly after treating oxygen-containing flue gas.
[0097] from Figure 1It can be seen that the metal particles are evenly dispersed in the carrier. The average particle size before and after the reaction is 16.92nm and 16.59nm, respectively, which remains almost unchanged. This shows that Ni9Cu1-CaZr can effectively inhibit the sintering of Ni and thus has better resistance to coke deposition. At relatively high temperatures, the microstructure of Ni9Cu1-CaZr changes less, which is undoubtedly related to its excellent cycle stability.
[0098] 2. Influence of DRM performance and Cu content
[0099] The experimental results of CO2 capture coupled with methane dry reforming in simulated oxygen-containing flue gas in Examples 1 to 3 and Comparative Example 1 are recorded in Tables 1 and Figure 2 middle.
[0100] Table 1 Comparison of single cycle performance of different dual-functional materials
[0101]
[0102] According to the data in Table 1, the CO2 capture capacity of the four groups of materials modified by zirconium oxide is about 9mmol / g. DFMs , while the sample without zirconia has a higher CO2 capture capacity due to its higher CaO content in the carrier; in addition, the CO2 conversion rate is also close to 100%, indicating that the CO2 escape rate is extremely low at 600℃. At the same time, due to the significant improvement of Cu on the reducibility of the dual-functional material, the in-situ delay phenomenon is suppressed ( Figure 2 ), and when Ni:Cu=9:1, the CH4 conversion rate was significantly improved, increasing by about 13%. When the Cu content was further increased, the CH4 conversion rate gradually decreased, and the total output (H2+CO) also decreased slightly. This is due to the decrease in the active component Ni, which leads to the decrease in performance. It can be seen that the Cu content is also an important factor affecting the catalytic performance. For the above four sets of data, the H2 / CO ratio of Example 1 is lower, indicating that the methane cracking side reaction (Formula 4) is weaker at this time, reducing the formation of carbon deposits, thereby effectively inhibiting the deactivation phenomenon caused by the covering of the catalyst active sites by carbon deposits.
[0103] CH4→C+2H2, ΔH 298K = +75 kJ·mol -1 (4)
[0104] 3. Influence of temperature
[0105] Based on the results in "2. DRM phenomenon and influence of Cu content", Example 1 with a Ni:Cu molar ratio of 9:1 can have the best performance while suppressing the in-situ delay in the conversion stage. On this basis, the inventors selected Example 1 and Comparative Example 1 without Cu doping to explore the effect of temperature on the activity of the dual-functional material.
[0106] The reaction process and conditions are:
[0107] (1) Heating stage: N2 condition, heating from room temperature to target temperature (625℃ / 650℃), heating rate 5℃ / min;
[0108] (2) Pre-reduction stage: 10% H2, N2 as balance gas, reaction time 120 min;
[0109] (3) N2 purge for 5 min;
[0110] (4) CO2 capture stage: 10% CO2, 6.7% O2, nitrogen as balance gas, reaction time 60 min;
[0111] (5) N2 purge for 5 min;
[0112] (6) Methane dry reforming stage: 2.5% CH4, reaction time 180 min;
[0113] (7) N2 purge for 5 min.
[0114] The total flow rate is 100 mL / min. The test results are shown in Table 2 and Figure 3 .
[0115] Table 2 Effect of temperature on single cycle performance of dual-function materials
[0116]
[0117] observe Figure 3 The results in Table 2 show that: the higher the temperature, the faster the reaction rate, and the entire reaction time is greatly reduced; at the same time, because the reaction activity of active hydrogen is stronger at high temperature, the delay time will also be shortened, that is, the reduction time of NiO is shortened, so the conversion rate of CH4 has been greatly improved. At different temperatures, Ni9Cu1-CaZr can effectively inhibit the occurrence of the delay phenomenon, and show better conversion rate and H2 / CO ratio under the same working conditions, proving that the addition of Cu can not only inhibit the in-situ delay phenomenon caused by oxygen-containing flue gas by improving the reducibility of the material, thereby improving the conversion performance, but also effectively inhibit carbon deposition and improve the stability of the material.
[0118] 4. Cycle stability
[0119] Based on the results in "2. DRM phenomenon and influence of Cu content", Example 1 with a Ni:Cu molar ratio of 9:1 can have the best performance while suppressing the in-situ delay in the conversion stage. On this basis, the inventors selected Example 1 and Comparative Example 1 without Cu doping to explore the cycle stability.
[0120] The reaction process and conditions are:
[0121] (1) Heating stage: N2 condition, from room temperature to 650°C, heating rate 5°C / min;
[0122] (2) Pre-reduction stage: 10% H2, N2 as balance gas, reaction time 120 min;
[0123] (3) Heating from 600°C to 650°C in N2 atmosphere at a rate of 5°C / min;
[0124] (4) CO2 capture stage: 10% CO2, 6.7% O2, N2 as balance gas, reaction time 60 min;
[0125] (5) N2 purge for 5 min;
[0126] (6) Methane dry reforming stage: 2.5% CH4, reaction time 180 min;
[0127] (7) N2 purge for 5 min.
[0128] The total flow rate of the whole process is 100 mL / min. After the process is performed once, steps (4) to (7) are repeated 4 times. The test results are shown in Table 3.
[0129] Table 3 Cyclic performance test table of dual-functional materials From Table 3, it can be seen that the CO production of the two groups of dual-functional materials is similar, but Example 1 shows better anti-carbon deposition performance because its H2 / CO is lower. In addition, the production of Example 1 decays less in 5 cycles, indicating that it has better cycle stability at high temperatures.
[0130] In summary, the dual-functional material prepared by the present invention has excellent performance in the process of oxygen-containing flue gas CO2 capture coupled with methane dry reforming. It not only effectively suppresses the delay in the conversion stage, improves the conversion rate of CH4, and suppresses the occurrence of methane cracking side reactions, but also has a stable microstructure, improved anti-carbon deposition performance, excellent stability at high temperatures, and good industrial application prospects.
Claims
1. Application of dual-functional materials for carbon dioxide capture coupled with methane dry reforming in oxygen-containing flue gas treatment, characterized in that: The dual-function material is a copper-modified nickel / calcium oxide composite material, and the dual-function material can suppress in-situ delay phenomenon and carbon deposition.
2. The use according to claim 1, characterized in that The dual-functional material is used in oxygen-containing flue gas treatment: at a temperature of 600° C., the conversion rate of carbon dioxide is 92-97%, the conversion rate of methane is 42-57%, and the H2 / CO ratio is 2.35-2.
36.
3. The use according to claim 1 or 2, characterized in that: The preparation method of the dual-functional material comprises: dissolving copper salt, nickel salt and calcium salt in water, adding anhydrous citric acid, stirring until the solution changes into a gel state, drying and calcining to obtain a copper-modified nickel / calcium oxide composite material.
4. The use according to claim 1, characterized in that The dual-function material is a nickel / calcium oxide composite material modified by copper and zirconium oxide, and the dual-function material can suppress in-situ delay phenomenon and carbon deposition.
5. The use according to claim 4, characterized in that In the treatment of oxygen-containing flue gas, the bifunctional material has the following characteristics: at a temperature of 600° C., the conversion rate of carbon dioxide is 98-99%, the conversion rate of methane is 44-55%, and the H2 / CO ratio is 2.00-2.12; after five cycles at a temperature of 650° C., the conversion rate of methane is 66.44%.
6. The use according to claim 4 or 5, characterized in that The preparation method of the dual-functional material comprises: dissolving copper salt, zirconium salt, nickel salt and calcium salt in water, adding anhydrous citric acid, stirring until the solution changes into a gel state, drying and calcining to obtain a copper and zirconium oxide modified nickel / calcium oxide composite material.
7. The use according to claim 6, characterized in that The copper salt, zirconium salt, nickel salt and calcium salt are copper nitrate, zirconium nitrate, nickel nitrate and calcium nitrate respectively.
8. The use according to claim 6, characterized in that The molar ratio of the nickel salt to the copper salt is (1-9):
1.
9. The use according to claim 6, characterized in that The sum of the molar amounts of the copper salt, zirconium salt, nickel salt and calcium salt is a mol, the molar amount of the anhydrous citric acid is a mol, and the molar amount of the water is 30a-45a mol.
10. The use according to claim 6, characterized in that The stirring temperature is 85-100° C.; the drying temperature is 120-140° C.; and the drying time is 8-24 h.
11. The use according to claim 6, characterized in that The calcination temperature is 650-750° C., the calcination time is 3-5 h, and the calcination heating rate is 4-6° C. / min.
Citation Information
Patent Citations
Preparation method and application of catalyst for hydrogen production through methane and carbon dioxide dry reforming
CN113522293A
Bifunctional catalyst applied to integration of CO2 capture and methanation in flue gas
CN113634257A
Preparation method and application of catalyst for preparing synthesis gas by coupling calcium cycle carbon dioxide capture and methane dry reforming
CN115090291A
Porous adsorption and catalysis bifunctional material as well as preparation method and application thereof
CN115445622A
Carbon dioxide adsorption-catalysis bifunctional material as well as preparation method and application thereof
CN117463343A
Cited By
Self-regeneration perovskite / alkaline earth metal oxide composite difunctional material and preparation and application thereof
CN120479444A