Catalyst Mn1-xCuxO2 / rGO for removing formaldehyde at room temperature and preparation method of catalyst Mn1-xCuxO2 / rGO

By in situ generating copper-doped manganese oxide on reduced graphene oxide, the problem of insufficient performance and stability of manganese-based oxide catalysts at room temperature is solved, and efficient formaldehyde catalytic oxidation and cycling performance is achieved, suitable for high-quality high-quality Humidity conditions.

CN118874485APending Publication Date: 2024-11-01SHANGHAI YOULAN SCI CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410996179.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing manganese-based oxide catalysts have poor formaldehyde catalytic oxidation performance and stability at room temperature, and are prone to photogenerated electron hole recombination and nanomaterial agglomeration, resulting in low catalytic activity and poor cycle performance.

Method used

Copper-doped manganese oxide (Mn1-xCuxO2) was generated in situ on reduced graphene oxide by solution precipitation method. The pH value and calcination temperature were adjusted by alkaline solution to form copper-doped manganese-based oxide and reduced graphene oxide. Complex, avoid agglomeration and improve catalytic activity.

Benefits of technology

The formaldehyde elimination efficiency and circulation performance of the catalyst are significantly improved, and efficient room-temperature formaldehyde catalytic oxidation is achieved, and good performance is maintained under high humidity conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004960274710000071
    Figure BDA0004960274710000071
  • Figure BDA0004960274710000091
    Figure BDA0004960274710000091
  • Figure BDA0004960274710000111
    Figure BDA0004960274710000111
Patent Text Reader

Abstract

The invention discloses a catalyst Mn1-xCuxO2 / rGO for removing formaldehyde at room temperature and a preparation method of the catalyst Mn1-xCuxO2 / rGO. A phase B precursor is generated in situ and loaded on a phase A, and then is roasted to form a phase B; the phase A is reduced graphene oxide powder, the phase B is copper-doped manganese oxide Mn1-xCuxO2, and x is more than 0.003 and less than or equal to 0.1; and the mass fraction of the Mn < 1-x > Cu < x > O < 2 > in the Mn < 1-x > Cu < x > O < 2 > / rGO is 10%-70%. Through copper doping, electrons are more easily captured in a d orbit, so that recombination of photo-induced electron holes is reduced, and the catalytic activity is effectively improved; mn1-xCuxO2 is compounded with rGO, so that the agglomeration of manganese oxide during catalytic reaction can be avoided, and the cycle performance is improved; the rGO is good in conductivity, is beneficial to electron transmission, is beneficial to regeneration of Mn1-xCuxO2 after catalytic reaction, and improves the cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of formaldehyde removal catalysts, and particularly relates to a room temperature formaldehyde removal catalyst Mn 1-x Cu x O2 / rGO and preparation method thereof. Background Art

[0002] Formaldehyde (HCHO) is the most common and serious indoor air pollutant. It affects the upper respiratory tract and lungs, causes liver function, immune function and nervous system abnormalities, and even induces cancer in severe cases. It is extremely harmful to human health. Therefore, the elimination of indoor formaldehyde gas has received more and more attention.

[0003] Studies have shown that room temperature catalytic oxidation technology is one of the most efficient technologies for purifying formaldehyde, and catalytic materials are the core factors that determine the performance of formaldehyde catalytic oxidation elimination. Therefore, it is very important to find a catalytic material with excellent performance.

[0004] Compared with other non-precious metals, manganese-based oxides have multiple valence states and different crystal phases, excellent catalytic performance and strong oxidation ability, and are a catalytic material with great application prospects. At present, the application research of manganese-based oxides in formaldehyde purification has made good progress. For example, patent document CN117398992A discloses a method for preparing a manganese dioxide catalyst for catalytic decomposition of formaldehyde, which mainly comprises Mn 2+ The method is prepared by oxidizing an inorganic salt, then adding an alkali solution to adjust the pH, separating the solid and the liquid, and drying. The obtained manganese dioxide catalyst has a very good formaldehyde catalytic decomposition effect at a high temperature of 85°C, which can reach up to 99% or more. However, the formaldehyde catalytic decomposition effect is poor under relatively low temperature conditions. In addition, the formaldehyde catalytic decomposition performance of the manganese dioxide catalyst still has room for improvement under the conditions of high formaldehyde space velocity and low concentration.

[0005] Many researchers have tried different approaches. For example, patent document CN117816151A discloses a manganese dioxide catalyst for decomposing formaldehyde. The crystal structure of the catalyst is delta-MnO2 type, and the specific surface area of ​​the catalyst is greater than or equal to 50 m 2 / g; manganese salt and potassium salt are used as raw materials, the molar ratio of K to Mn is 0.05-0.25, and hydrothermal treatment is carried out at 80-200°C for 1-24h. However, the document does not mention the cyclic reaction, does not verify the persistence of activity, and has limitations in practical application.

[0006] Patent document CN107754785A discloses a graphene-manganese oxide composite catalyst for low-temperature catalytic oxidation of formaldehyde, including graphene nanosheets and manganese oxide nanosheets supported on the graphene nanosheets; including the following steps: 1) dispersing graphene oxide in deionized water, and then ultrasonically dispersing for 10-60 minutes to obtain a graphene oxide dispersion; moving the graphene oxide dispersion into a reactor, sealing and reacting at 80-200°C for 6-18 hours, centrifuging, washing and freeze-drying after the reaction to obtain graphene nanosheets; 2) mixing the graphene nanosheets and potassium permanganate aqueous solution, and then stirring the reaction at room temperature for 10-24 hours, washing, filtering and freeze-drying after the reaction to obtain a graphene-manganese oxide composite catalyst. However, the document does not mention the phenomenon that the manganese oxide catalyst is deactivated at high humidity, and no humidity verification is performed.

[0007] Patent document CN117427630A discloses a δ-MnO2-GO catalyst and its preparation method and application in formaldehyde degradation at room temperature, including the following steps: S1. Prepare 1.6-10g / L graphene oxide aqueous solution, add manganese sulfate to the graphene oxide solution, so that the concentration of manganese sulfate is 50-300g / L, and obtain a mixed solution; S2. Add a potassium permanganate aqueous solution with a concentration of 30-60g / L to the mixed solution of S1, stir for 30min, age at room temperature for more than 12h, and dry. The document uses low-amount GO doping to significantly limit the growth of manganese dioxide nanosheets and create abundant mass transfer channels. The δ-MnO2-GO catalyst presents a unique two-dimensional crown structure, and the δ-MnO2 nanorods with a two-dimensional coral-like hierarchical pore structure are uniformly dispersed on the planar structure of GO. Graphene oxide has many surface active groups and is more likely to absorb moisture, which has a great influence on the catalytic activity of manganese oxide, but the document does not mention the influence of humidity and its influence on catalytic activity.

[0008] Patent document CN118237010A discloses a composite catalyst for efficient formaldehyde elimination, wherein the raw materials for preparation include phase A and phase B, wherein phase A includes activated carbon powder, and the specific surface area of ​​the activated carbon powder is greater than 1000m 2 / g, mesh size greater than 300 mesh; phase B includes a manganese source compound and an alkaline solution; the manganese source compound includes one of manganese sulfate, manganese acetate, manganese chloride or manganese oxalate, and the alkaline solution includes one of potassium hydroxide solution, sodium hydroxide solution, potassium carbonate solution, potassium bicarbonate solution, sodium carbonate solution or sodium bicarbonate solution; the document is prepared by hydrophilic modification of activated carbon powder and reaction with a manganese source compound and an alkaline solution. However, the synergistic effect of activated carbon powder and manganese oxide is not reflected in the document, and only the structure of activated carbon is used to avoid the agglomeration of manganese oxide, which is not very helpful for the catalytic activity and regeneration of manganese oxide, so the cyclicity of room temperature catalytic oxidation of formaldehyde still needs to be improved.

[0009] Patent document CN107790152A discloses a catalyst for removing harmful gases, its preparation method and application. The catalyst uses activated carbon as a carrier, and metal oxides accounting for 4%-25% of the total mass of the catalyst are loaded on the activated carbon. The metal oxides are copper oxide and manganese oxide, and the molar ratio of copper oxide to manganese oxide is 3:1-1:5; the copper in the copper oxide is basically +2 valence, and there are manganese monoxide, manganese dioxide and other situations in manganese oxide, but the calcination process is mainly manganese dioxide. The document immerses the activated carbon in an aqueous solution containing copper salt and manganese salt for 20-32 hours, directly dries after the immersion, and then calcines the dried solid under a protective atmosphere at 400℃-600℃ for 3-10 hours to obtain a catalyst. However, in this preparation method, the copper salt and manganese salt in the activated carbon are limited to the amount adsorbed in the pore size of the activated carbon, resulting in the copper and manganese elements being unable to achieve a very high retention rate, and also making it unable to achieve a higher catalytic effect. If an alkaline solution is added to generate precipitation based on the literature, the pores of the activated carbon will be blocked, resulting in a decrease in the specific surface area and active sites of the activated carbon, which will also reduce the effectiveness of the catalyst.

[0010] The above literature still has the problem of poor performance and stability of manganese-based oxides in catalytic oxidation of formaldehyde at room temperature. The main reason is that the photogenerated electron holes of manganese-based oxides are easy to recombine, affecting the catalytic activity. In addition, nanomaterials are easy to agglomerate, resulting in reduced performance and stability. Summary of the invention

[0011] The purpose of the present invention is to provide a room temperature formaldehyde removal catalyst Mn 1-x Cu x O2 / rGO and its preparation method are used to solve the problems of low catalytic activity and poor cycle performance caused by easy recombination and agglomeration of photogenerated electrons and holes in the prior art.

[0012] The purpose of the present invention is achieved through the following technical solutions:

[0013] A room temperature formaldehyde removal catalyst Mn of the present invention 1-x Cu x The preparation method of O2 / rGO is characterized by comprising the following steps:

[0014] S1, dispersing reduced graphene oxide in water, stirring to make it uniform, and obtaining a reduced graphene oxide solution;

[0015] S2, adding a manganese source compound and a copper source compound to the reduced graphene oxide solution respectively, and stirring to obtain a mixed solution;

[0016] S3, adding an alkaline solution dropwise to the mixed solution, adjusting the pH value of the solution to 9-12, and stirring to perform a precipitation reaction;

[0017] S4, filtering, washing, and drying the reaction product to obtain reduced graphene oxide loaded with the B-phase precursor;

[0018] S5, grinding the reduced graphene oxide loaded with the B phase precursor, placing it in a muffle furnace for calcining, using nitrogen as a protective gas during calcination, and then obtaining the room temperature formaldehyde removal catalyst Mn 1-x Cu x O2 / rGO;

[0019] The reduced graphene oxide (usually abbreviated as rGO) is a multilayer graphene material obtained by reducing the oxidized functional groups of graphene oxide or graphite oxide, with 2 to 5 layers and a specific surface area of ​​≥100m 2 / g, the larger the specific surface area, the better the effect, and the better the hydrophilicity, the better the effect; preferably, the reduced graphene oxide obtained by the thermal expansion hydrogen reduction method; for example, the DZ-696 brand product produced by Kerui Nano (Guangdong) Co., Ltd.;

[0020] The manganese source compound is at least one of manganese sulfate, manganese acetate, manganese nitrate, manganese chloride or manganese oxalate; the copper source compound is at least one of copper sulfate, copper nitrate, copper acetate and copper chloride; the alkaline solution is at least one of potassium hydroxide solution, sodium hydroxide solution, potassium carbonate solution, potassium bicarbonate solution, sodium carbonate solution or sodium bicarbonate solution with a mass fraction of 1% to 15%; the B phase precursor is formed by precipitation reaction of a manganese source compound and a copper source compound with an alkaline solution.

[0021] Preferably, the mass concentration of the manganese source compound in the mixed solution is 0.5% to 2%, and the mass concentration of the copper source compound in the mixed solution is 0.005% to 2%; and the precipitation reaction time is 1 to 5 hours.

[0022] Preferably, the precipitation reaction time in step S3 is 1 to 5 hours.

[0023] Preferably, the drying temperature of step S4 is 20-100° C., and the drying time is 1-6 hours.

[0024] Preferably, the calcination temperature in step S5 is 200-600° C., and the calcination time is 1-6 hours.

[0025] The above-mentioned solution concentration, pH value, precipitation time, calcination temperature and calcination time will all affect the crystal form (β-MnO2, γ-MnO2, α-Mn2O3, γ-Mn2O3, α-Mn3O4 and Mn5O8) of the prepared copper-doped manganese-based oxide and the valence state (+Ⅱ, +Ⅲ, +Ⅳ) of the manganese atoms, thereby changing the formaldehyde elimination performance parameters of the final product.

[0026] The room temperature formaldehyde removal catalyst Mn 1-x Cu x Preparation method of O2 / rGO for preparing room temperature formaldehyde removal catalyst Mn 1-x Cu x O2 / rGO; characterized in that the B phase precursor is in-situ generated and loaded on the A phase, and then calcined to form the B phase; the A phase is reduced graphene oxide powder; the B phase is copper-doped manganese oxide Mn 1-x Cu x O2 and 0.003<x≤0.1, preferably x=0.01~0.1, if x is too large, the crystal form will change and the catalytic activity will be greatly reduced;

[0027] The Mn 1-x Cu x O2 in the Mn 1-x Cu x The mass fraction of O2 / rGO is 10% to 70%, preferably 20% to 60%.

[0028] Compared with the prior art, the present invention has the following advantages:

[0029] The present invention adopts a solution precipitation method to directly generate Mn and Cu elements in situ on the surface of reduced graphene oxide, which not only abandons the pore size and porosity limitations of activated carbon, but also firmly fixes Mn and Cu elements by reducing the functional groups remaining on the surface of graphene oxide, thereby having a synergistic effect with the reduced graphene oxide and greatly increasing the catalytic effect; through copper doping, it is easier to capture electrons in the d orbit, reduce the recombination of photogenerated electron holes, and effectively improve the catalytic activity; Mn 1- x Cu x O2 and rGO composite can avoid the agglomeration of manganese oxide during catalytic reaction and increase the cycle performance; rGO has good conductivity, which is conducive to electron transmission and helps Mn 1-x Cu x Regeneration after O2 catalytic reaction increases cycle performance. DETAILED DESCRIPTION

[0030] Those skilled in the art should realize that the present embodiment is only used to illustrate the present invention, but not to limit the present invention.

[0031] The raw materials used in the present invention are all commercially available products.

[0032] Example 1: Formaldehyde elimination test

[0033] A room temperature formaldehyde removal catalyst Mn 1-x Cu x The preparation method of O2 / rGO comprises the following steps:

[0034] S1. Disperse 2 g of reduced graphene oxide in 150 mL of water and stir for 1 h to make it uniform to obtain a reduced graphene oxide solution;

[0035] S2, adding 1.26 g of MnCl2 and 0.07 g of CuCl2 to the reduced graphene oxide solution, respectively, and stirring to obtain a uniform mixed solution of MnCl2, CuCl2 and reduced graphene oxide;

[0036] S3, dropwise adding Na2CO3 solution to the mixed solution, adjusting the pH value of the solution to 9.5, stirring for precipitation reaction until no more precipitate is generated;

[0037] S4, filtering and washing the reaction product, and drying it by air blast at 100° C. to obtain reduced graphene oxide loaded with the B phase precursor;

[0038] S5. Grind and break up the reduced graphene oxide loaded with the B-phase precursor, place it in a muffle furnace, and calcine it at 400° C. for 4 h under nitrogen protection to obtain 30 wt% (Mn 0.95 Cu 0.05 O2 accounts for Mn 0.95 Cu 0.05 O2 / rGO mass fraction, the same below) of room temperature formaldehyde removal catalyst Mn 0.95 Cu 0.05 O2 / rGO, with a yield of 72.5%.

[0039] Comparative Example 1

[0040] Commercially available MnO2 samples.

[0041] Comparative Example 2

[0042] The catalyst of Example 1 of document CN118237010A.

[0043] Test Example 1

[0044] Weigh 0.10 g of the room temperature formaldehyde removal catalyst Mn prepared in Example 1. 0.95 Cu 0.05 O2 / rGO, placed in a quartz tube fixed bed reactor with an inner diameter of 8 mm; the reaction gas was 0.55 mg / m 3 Formaldehyde gas and 100% high-purity air, the reaction gas flow rate is 100mL / min; at a temperature of 30°C and a humidity of 50%, the reaction is carried out continuously for 5 times (each reaction lasts 20min, the same below); the formaldehyde residue in the tail gas is determined by phenol reagent spectrophotometry, and the performance of the catalyst in removing formaldehyde from the air is shown in Table 1.

[0045] Under the same conditions as Example 1, 0.10 g of Comparative Example 1 and Comparative Example 2 were respectively placed in a quartz tube fixed bed reactor with an inner diameter of 8 mm and reacted continuously for five times. The formaldehyde residue in the tail gas was determined by phenol reagent spectrophotometry, and the performance results of the catalyst in removing formaldehyde from the air are shown in Table 1.

[0046] Table 1 Test results of Example 1 and Comparative Examples 1-2

[0047]

[0048] The results show that compared with the commercially available MnO2 and the catalyst in the document CN118237010A, the room temperature formaldehyde removal catalyst Mn prepared in Example 1 1-x Cu x O2 / rGO (x = 0.05), 30wt% Mn 1-x Cu x The O2 / rGO catalyst still achieved a formaldehyde removal efficiency of more than 99%, and had good formaldehyde removal performance.

[0049] Example 2: High air velocity, high humidity, low concentration formaldehyde elimination test

[0050] A room temperature formaldehyde removal catalyst Mn 1-x Cu x The preparation method of O2 / rGO comprises the following steps:

[0051] S1. Disperse 0.6 g of reduced graphene oxide in 150 mL of water and stir for 1 h to make it uniform to obtain a reduced graphene oxide solution;

[0052] S2, adding 1.7 g of Mn(NO3)2 and 0.09 g of Cu(NO3)2 to the reduced graphene oxide solution, respectively, and stirring to obtain a uniform mixed solution of Mn(NO3)2, Cu(NO3)2 and reduced graphene oxide;

[0053] S3, adding NaOH solution dropwise to the mixed solution, adjusting the pH value of the solution to 9.5, stirring for precipitation reaction until no more precipitate is generated;

[0054] S4, filtering and washing the reaction product, and drying it by air blast at 100° C. to obtain reduced graphene oxide loaded with the B phase precursor;

[0055] S5, grinding and breaking up the reduced graphene oxide loaded with the B phase precursor, placing it in a muffle furnace, and calcining it at 400° C. for 4 h under nitrogen protection to obtain a 60 wt% room temperature formaldehyde removal catalyst Mn 0.95 Cu 0.05 O2 / rGO, with a yield of 66.7%.

[0056] Test Example 2

[0057] Weigh 0.10 g of the room temperature formaldehyde removal catalyst Mn prepared in Example 2 0.95 Cu 0.05 O2 / rGO, placed in a quartz tube fixed bed reactor with an inner diameter of 8 mm; the reaction atmosphere was 0.28 mg / m 3 Formaldehyde gas and 100% high-purity air, the reaction gas flow rate is 500mL / min; the humidity inside the reactor is changed by the bubbling method, and the decomposition efficiency is tested at a temperature of 30°C and humidity levels of 50%, 70%, and 90%RH, respectively, and the reaction is repeated 5 times (each reaction lasts 20min, the same below); the formaldehyde residue in the tail gas is determined by phenol reagent spectrophotometry, and the performance of the catalyst in eliminating formaldehyde in the air is shown in Table 2.

[0058] 0.10 g of Comparative Example 1 and Comparative Example 2 were weighed and placed in a quartz tube fixed bed reactor with an inner diameter of 8 mm; the reaction was continued for five times under the same conditions as Example 2 at a temperature of 30° C. and a humidity level of 70% RH. The formaldehyde residue in the tail gas was measured by phenol reagent spectrophotometry, and the performance of the catalyst in removing formaldehyde from the air was obtained, as shown in Table 2.

[0059] Table 2 Test results of Example 2 and Comparative Examples 1-2

[0060]

[0061] The results show that compared with the commercially available MnO2 and the catalyst in the literature CN118237010A, the room temperature formaldehyde removal catalyst Mn prepared in Example 2 0.95 Cu 0.05 Under high humidity conditions with a humidity level of 70% RH, the room temperature formaldehyde removal catalyst Mn prepared in Example 2 1-x Cu x O2 / rGO still achieved a formaldehyde removal efficiency of more than 98%.

[0062] Examples 3-5: Test on the effect of changing the doping amount on formaldehyde removal performance

[0063] A room temperature formaldehyde removal catalyst Mn 1-x Cu x The preparation method of O2 / rGO comprises the following steps:

[0064] S1. Disperse 0.6 g of commercially available graphene oxide (GO) in 150 mL of water and stir for 1 h to make it uniform to obtain a reduced graphene oxide solution;

[0065] S2, Example 3: 1.25g of MnCl2 and 0.01g of CuCl2, Example 4: 1.2g of MnCl2 and 0.07g of CuCl2, Example 5: 1.13g of MnCl2 and 0.14g of CuCl2 are added to the reduced graphene oxide solution; Examples 3 to 5 are stirred separately to obtain three different uniform mixed solutions of MnCl2, CuCl2 and reduced graphene oxide, and the corresponding doping ratios are: Mn 0.99 Cu 0.01 O2 / rGO, marked as Example 3-0.01; Mn 0.95 Cu 0.05 O2 / rGO, marked as Example 4-0.05; Mn 0.9 Cu 0.1 O2 / rGO, labeled as Example 5-0.1;

[0066] S3, respectively adding Na2CO3 solution to the mixed solutions of Examples 3 to 5, adjusting the pH value of the solution to 9.5, stirring for precipitation reaction until no more precipitate is generated;

[0067] S4, filtering and washing the reaction products of Examples 3 to 5 respectively, and drying them by air blast at 100° C. to obtain reduced graphene oxide loaded with a B-phase precursor;

[0068] S5. Grind and break up the reduced graphene oxide loaded with the B-phase precursor of Examples 3 to 5, place them in a muffle furnace, and calcine them at 400° C. for 4 h under nitrogen protection to obtain a 60 wt% room temperature formaldehyde removal catalyst Mn 1- x Cu x O2 / rGO, with yields of 66.7%, 66.5% and 66.8%.

[0069] Comparative Example 3 (without Cu doping)

[0070] Take 0.6g of reduced graphene oxide and disperse it in 150mL of water, and stir for 1h to make it uniform; then add 1.26g of MnCl2 and stir to obtain a uniform mixed solution of MnCl2 and reduced graphene oxide; add Na2CO3 solution dropwise to the above mixed solution, adjust the pH value of the solution to 9.5, and stir to carry out precipitation reaction; filter and wash the reaction product, and blow dry it at 100°C to obtain a precipitated product; grind the precipitated product, put it in a muffle furnace, and calcine it at 400°C for 4h under nitrogen protection to obtain 60wt% (the mass fraction of MnO2 in MnO2 / rGO) of MnO2 / rGO composite catalyst with a yield of 70%.

[0071] Test Example 3

[0072] 0.10 g of the room temperature formaldehyde removal catalysts prepared in Examples 3 to 5 and Comparative Example 3 were weighed and placed in a quartz tube fixed bed reactor with an inner diameter of 8 mm; the reaction atmosphere was 0.28 mg / m 3 Formaldehyde gas and 100% high-purity air, the reaction gas flow rate is 500mL / min; under the high humidity conditions of temperature 30°C and humidity 70%RH, the reaction is carried out continuously for 5 times (each reaction for 20min); the formaldehyde residue in the tail gas is determined by phenol reagent spectrophotometry, and the performance results of the catalyst in eliminating formaldehyde in the air are shown in Table 3.

[0073] Table 3 Test results of Examples 3 to 5 and Comparative Example 3

[0074]

[0075] It can be seen from Table 3 that the catalysts Mn prepared in Examples 3 to 5 1-x Cu x The formaldehyde elimination efficiency of the O2 / GO catalyst was maintained above 76%. The formaldehyde elimination efficiency of the 60wt% MnO2 / rGO composite catalyst prepared in Comparative Example 3 was maintained below 66.1%, which was lower than the efficiency of the composite catalyst prepared with MnCl2 and CuCl2 as raw materials. This indicates that the doping of copper ions has an effect on the prepared Mn 1-x Cu x It has an important influence on the catalytic performance of O2 / rGO composite catalyst.

[0076] The 60wt% Mn prepared in Example 2 0.95 Cu 0.05 O2 / rGO was reacted continuously for 5 times under the same conditions as in Example 3, and the formaldehyde elimination efficiency could reach more than 99%, indicating that excessive doping of copper element (x exceeding 0.1) is harmful to the catalytic effect of the catalyst.

Claims

1. A room temperature formaldehyde removal catalyst Mn 1-x Cu x The preparation method of O2 / rGO is characterized in that: The steps include: S1, dispersing reduced graphene oxide in water, stirring to make it uniform, and obtaining a reduced graphene oxide solution; S2, adding a manganese source compound and a copper source compound to the reduced graphene oxide solution respectively, and stirring to obtain a mixed solution; S3, adding an alkaline solution dropwise to the mixed solution, adjusting the pH value of the solution to 9-12, and stirring to perform a precipitation reaction; S4, filtering, washing, and drying the reaction product to obtain reduced graphene oxide loaded with the B-phase precursor; S5, grinding the reduced graphene oxide loaded with the B phase precursor, placing it in a muffle furnace for calcining, using nitrogen as a protective gas during calcination, and then obtaining the room temperature formaldehyde removal catalyst Mn 1-x Cu x O2 / rGO.

2. The preparation method according to claim 1, characterized in that: The reduced graphene oxide is a multilayer graphene material obtained by reducing the oxidized functional groups of graphene oxide or graphite oxide, with 2 to 5 layers and a specific surface area of ​​≥100m 2 / g.

3. The preparation method according to claim 1, characterized in that: The manganese source compound is at least one of manganese sulfate, manganese acetate, manganese nitrate, manganese chloride or manganese oxalate; the copper source compound is at least one of copper sulfate, copper nitrate, copper acetate and copper chloride; the alkaline solution is at least one of potassium hydroxide solution, sodium hydroxide solution, potassium carbonate solution, potassium bicarbonate solution, sodium carbonate solution or sodium bicarbonate solution with a mass fraction of 1% to 15%; the B phase precursor is formed by precipitation reaction of a manganese source compound and a copper source compound with an alkaline solution.

4. The preparation method according to claim 1, characterized in that: The mass concentration of the manganese source compound in the mixed solution is 0.5% to 2%, and the mass concentration of the copper source compound in the mixed solution is 0.005% to 2%; the precipitation reaction time is 1 to 5 hours.

5. The preparation method according to claim 1, characterized in that: The precipitation reaction time in step S3 is 1 to 5 hours.

6. The preparation method according to claim 1, characterized in that: The drying temperature of step S4 is 20-100° C., and the drying time is 1-6 hours.

7. The preparation method according to claim 1, characterized in that: The calcination temperature in step S5 is 200-600° C., and the calcination time is 1-6 hours.

8. A room temperature formaldehyde removal catalyst Mn prepared by the preparation method according to any one of claims 1 to 7 1-x Cu x O2 / rGO, characterized in that The B phase precursor is in-situ generated and loaded on the A phase, and then calcined to form the B phase; the A phase is reduced graphene oxide powder, and the B phase is copper-doped manganese oxide Mn 1-x Cu x O2 and 0.003<x≤0.1; the Mn 1-x Cu x O2 in the Mn 1- x Cu x The mass fraction in O2 / rGO is 10% to 70%.

9. The room temperature formaldehyde removal catalyst Mn according to claim 8 1-x Cu x O2 / rGO, characterized in that The Mn 1-x Cu x In O2, x=0.01~0.

1.

10. The room temperature formaldehyde removal catalyst Mn according to claim 8 1-x Cu x O2 / rGO, characterized in that The Mn 1- x Cu x O2 in the Mn 1-x Cu x The mass fraction in O2 / rGO is 20% to 60%.

Citation Information

Patent Citations

  • Composite catalyst for purifying indoor formaldehyde and preparation method of composite catalyst

    CN102198405A

  • Copper-doped manganese dioxide catalyst and preparation method therefor

    CN105797741A

  • Gas-sensitive material for detecting low-concentration formaldehyde at room temperature and preparation method of gas-sensitive material and gas sensor

    CN107290389A

  • Graphene-manganese oxide composite catalyst for low-temperature catalytic oxidation of formaldehyde, and preparation method thereof

    CN107754785A

  • Binary composite material for removing aldehyde through visible light catalysis and preparation method of binary composite material

    CN114768786A