Preparation method and application of an organic matter-green rust composite photocatalyst
By preparing an organic matter-green rust composite photocatalyst, the problems of insufficient catalytic activity and stability of green rust were solved, achieving efficient and stable pollutant degradation, which is suitable for the remediation of soil and groundwater pollution.
Patent Information
- Application Number
- CN202410910947.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-07-09
AI Technical Summary
Green rust has low catalytic activity, low degradation efficiency and poor stability, making it difficult to meet the needs of pollutant remediation. It is also prone to deactivation under reducing conditions, which limits its application in soil and groundwater.
An organic matter-green rust composite photocatalyst was prepared by dissolving anhydrous FeCl3, organic matter, and sodium acetate trihydrate in an organic solvent. After treatment in a hydrothermal reactor, the catalyst was washed and dried. Subsequently, nano-Au and nano-Ag particles were alternately magnetron sputtered on the catalyst surface to form SPR effect hotspots, and an Al2O3 film was deposited to enhance stability and activity.
It improves the photocatalytic activity and stability of green rust, enabling it to slowly degrade pollutants under sunlight, achieving in-situ removal and green remediation of pollutants without the need for additional chemical agents.
Smart Images

Figure CN118874536B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of photocatalyst preparation technology, specifically to a method for preparing and applying an organic-rust composite photocatalyst. Background Technology
[0002] Green rust (GRs) is considered a highly promising in-situ remediation material. As one of the most active iron-bearing minerals found in oxygen-deficient soil layers, aquifers, and sedimentary layers of high-speed railways, it has a certain ability to degrade and remove recalcitrant organic pollutants in the environment under sunlight conditions. Moreover, it is green and environmentally friendly and will not have other adverse effects on the environment.
[0003] However, the current method of directly using green rust to remove pollutants still has the following shortcomings:
[0004] Low catalytic activity: Although it has been found that green rust can directly degrade organic pollutants, the degradation efficiency is low and the remediation time is long, which affects the pollution remediation effect and makes it difficult to meet the remediation needs; Poor stability: Green rust exists under reducing conditions. After contact with oxygen, it easily loses structural divalent iron (Fe(II)) and is transformed into low-activity iron minerals, which leads to catalyst deactivation and limits its long-distance transport in soil and groundwater.
[0005] Existing technologies related to rust mainly focus on adsorption and reduction. There is very little research on the direct photocatalytic degradation of organic pollutants by rust. There are no reports on the use of common organic matter to modify rust and apply it to in-situ photocatalytic degradation of pollutants. Summary of the Invention
[0006] To address the above problems, this invention provides a method for preparing an organic-rust-based composite photocatalyst, comprising the following steps:
[0007] S1. Dissolve anhydrous FeCl3, organic matter, and sodium acetate trihydrate in an organic solvent at a molar ratio of 20-27:1:64.5-87.4, and stir at 75-85℃ for 25-35 minutes to obtain a composite solution.
[0008] S2. Transfer the composite solution to a stainless steel hydrothermal reactor, seal it, and maintain it at 190-210℃ for 22-26 hours.
[0009] S3. After the reactor cools to room temperature, open the reactor and pour off the liquid substance on the top to obtain wet powder. Take out the wet powder and wash and dry it to obtain the organic matter-green rust composite photocatalyst.
[0010] Note: Maintaining the above temperature for 24 hours ensures the continuous progress of the reaction. Glycerol can undergo catalytic reforming at temperatures above 160°C; maintaining this temperature for 24 hours ensures effective catalytic reforming and guarantees the Fe... 3+ Reduced to Fe 2+ And the generation of lactic acid anions.
[0011] Further, in step S1, the organic matter is humic acid or fulvic acid;
[0012] Note: The above-mentioned organic matter is common in nature and can solve the current shortcomings of green rust in photocatalysis. On the one hand, it can improve the photocatalytic activity of green rust so that it can meet the removal targets and needs of pollutants. On the other hand, it has good stability and can further improve the environmental remediation potential of photocatalysts.
[0013] Further, in step S1, the organic solvent is glycerol;
[0014] Note: Glycerol can undergo catalytic reforming at a high temperature of 160℃ to produce hydrogen as an effective reducing agent. The produced hydrogen will partially reduce Fe. 3+ Reduced to Fe 2+ Meanwhile, the trisaccharide intermediate produced by glycerol after hydrogen production can undergo continuous rearrangement to generate lactate anions, which can then participate in subsequent synthesis processes.
[0015] Further, in step S3, the washing method is as follows: washing 3-5 times sequentially with anhydrous ethanol and ethanol solution; the ethanol solution is obtained by mixing deionized water and ethanol in a volume ratio of 1:1.
[0016] Explanation: A solution of anhydrous ethanol and deionized water effectively removes soluble impurities from the powder surface, such as unreacted raw materials, byproducts, and residual solvents. These impurities can affect the purity, stability, and performance of the powder. Simultaneously, it maintains the powder's dispersibility and prevents particle agglomeration during washing and drying. Ethanol's moderate volatility allows for gradual evaporation during drying, helping to control the drying rate and preventing cracking, agglomeration, or structural damage caused by rapid drying. Multiple washes further improve powder purity. By controlling the ratio of ethanol to deionized water, the wettability of the powder can be adjusted, which helps improve the dispersibility of catalyst particles in the support or reaction system. Good dispersibility increases the effective surface area of the catalyst, thereby enhancing catalytic activity.
[0017] Further, in step S3, the drying method is: drying in an oven at 55-65℃ for 10-12 hours;
[0018] Note: Appropriate drying temperature and time help stabilize the structure of the photocatalyst, reduce the possibility of structural deformation or damage, and effectively reduce the occurrence of agglomeration, thus maintaining the dispersibility and catalytic performance of the photocatalyst.
[0019] Furthermore, the organic matter-green rust composite photocatalyst is subjected to surface treatment before drying.
[0020] The surface treatment method is as follows: Nano-Au and nano-Ag particles are alternately magnetron sputtered onto the washed organic-green rust composite photocatalyst surface to obtain a base film with a thickness of 5-10 nm per layer. The sputtering range of the base film occupies 1 / 4 to 3 / 4 of the organic-green rust composite photocatalyst surface, and the total thickness of the base film is 2-5 μm. Then, a composite mixture is vapor-deposited onto the surface of the outermost base film using microwave plasma to obtain the outer shell layer. The nano-Au and nano-Ag particles have a particle size of 2-25 nm. The magnetron sputtering parameters are: substrate pressure of 2 × 10⁻⁶. -5 -5×10 -4 The film formation pressure is 0.3-0.8 Pa, the sputtering target power is 70-150 W; the vapor deposition parameters are: the deposition gas source is oxygen, the vapor deposition temperature is 1000-1200 W, the deposition pressure is 5-12 kPa, and the gas residence time is 0.5-1 s.
[0021] The composite mixture comprises, by mass percentage: 35-45% Al2O3 solution with a concentration of 0.5-1 mg / mL, 5-10% fluoroboron pyrrole dye, 15-20% surfactant, and the balance being organic solvent.
[0022] Explanation: Au and Ag nanoparticles exhibit surface plasmon resonance (SPR) effect, which can significantly enhance the light absorption capacity of photocatalysts in the visible light region. By alternately magnetron sputtering Au and Ag nanoparticles, SPR effect hotspots can be formed on the surface of the photocatalyst, thereby improving the activity of the photocatalyst. The deposition of Al2O3 film can protect the photocatalyst from environmental corrosion and provide additional photocatalytic active sites, further improving photocatalytic efficiency. The organic matter-green rust composite photocatalyst itself may have a certain spectral response range, but after being combined with fluoroboron pyrrole dye, the fluoroboron pyrrole dye can act as a sensitizer, absorbing visible light and transferring energy to the photocatalyst, thereby expanding the spectral response range of the photocatalyst and enabling it to absorb photons in a wider wavelength range.
[0023] Metal nanoparticles (Au and Ag) can be alternately prepared to form composite films with multiple functions, exhibiting high hardness, high wear resistance, and high corrosion resistance. The deposition of the outermost Al2O3 film can improve the dispersion and stability of the catalyst on the support, which helps to reduce catalyst shedding and improve the catalyst's lifespan. As a protective layer and electron transport layer, the Al2O3 film can promote the transfer of electrons from the photocatalyst surface to the metal nanoparticles or from the metal nanoparticles to the photocatalyst, thereby accelerating the photocatalytic reaction rate.
[0024] Furthermore, during magnetron sputtering, nitrogen gas is introduced at a flow rate of 25-30 sccm for blowing, and the process is carried out at a temperature of 100-200℃ for 50-200 seconds.
[0025] Note: Nitrogen blowing and temperature control can improve the interfacial properties between gold and silver nanofilms and the photocatalyst, promoting electron transport and photogenerated carrier separation. This helps reduce the recombination probability of electrons and holes, thus improving photocatalytic efficiency. Nitrogen blowing can also protect the photocatalyst surface, reducing oxidation or corrosion during sputtering. Furthermore, nitrogen can react with metal nanoparticles to form a nitride layer, further enhancing the stability of the photocatalyst.
[0026] The present invention also provides an application of an organic matter-green rust stabilized photocatalyst, which is used for photocatalytic degradation of bisphenol pollutants based on the above-mentioned preparation method of an organic matter-green rust stabilized photocatalyst.
[0027] Furthermore, the method for photocatalytic degradation of bisphenol pollutants is as follows: 45-55 mL of pollutants BPF and BPS are placed in a reaction tube, and then 18-22 mg of an organic matter-green rust composite photocatalyst is added. The tube is then irradiated with a 480-520 W xenon lamp under simulated solar conditions for 8-12 hours to complete the photodegradation experiment; wherein the xenon lamp wavelength is 350-780 nm and the light power density is 214 mW / cm². 2 .
[0028] The beneficial effects of this invention are:
[0029] (1) This invention will prepare a novel “organic matter-green rust composite photocatalyst” by combining common organic matter in nature (fulvic acid FA and humic acid HA) to solve the current shortcomings of green rust in photocatalysis. On the one hand, it will improve the photocatalytic activity of green rust so that it can meet the removal target and demand of pollutants. On the other hand, the composite material synthesized by this invention has better stability, further improving its environmental remediation potential. Importantly, this material does not require the addition of additional chemical agents and will not generate other additional pollution. It can be directly put into the contaminated site and can slowly degrade the target pollutants under sunlight, thus achieving in-situ removal and green remediation of pollutants.
[0030] (2) This invention performs surface treatment on the washed organic-green rust composite photocatalyst, and uses alternating magnetron sputtering of nano-Au particles and nano-Ag particles to form SPR effect hot spots on the surface of the photocatalyst, which effectively improves the activity of the photocatalyst. The alternating film formation method enhances the corrosion resistance and wear resistance of the photocatalyst. Then, the outer layer of the metal base film is deposited by vapor deposition. Organic dyes and Al2O3 are used to expand the spectral response range of the photocatalyst, enabling it to absorb photons in a wider wavelength range, thereby improving the stability and photocatalytic ability of the photocatalyst. Attached Figure Description
[0031] Figure 1 This is the BET diagram of the humic acid-green rust composite photocatalyst HA@GRs in Example 1 of the present invention;
[0032] Figure 2 This is the FTIR image of the humic acid-green rust composite photocatalyst HA@GRs in Example 1 of this invention;
[0033] Figure 3 This is the Raman diagram of the humic acid-green rust composite photocatalyst HA@GRs in Example 1 of this invention;
[0034] Figure 4 This is a SEM image of the humic acid-green rust composite photocatalyst HA@GRs in Example 1 of this invention;
[0035] Figure 5 This is the XRD pattern of the humic acid-green rust composite photocatalyst HA@GRs in Example 1 of this invention;
[0036] Figure 6 These are the EPR graphs of the humic acid-green rust composite photocatalyst HA@GRs in Example 1 of this invention and the superoxide radical detection in blank group 1;
[0037] Figure 7 These are the EPR images of the humic acid-green rust composite photocatalyst HA@GRs in Example 1 of this invention and the singlet oxygen detection in blank group 1;
[0038] Figure 8 These are the EPR graphs of the humic acid-green rust composite photocatalyst HA@GRs in Example 1 of this invention and the hydroxyl radical detection in the blank group 1;
[0039] Figure 9 This is a graph showing the degradation efficiency of bisphenol A and bisphenol F by the humic acid-green rust composite photocatalyst HA@GRs in Example 1 of this invention.
[0040] Figure 10This is the FTIR image of the fulvic acid-green rust composite photocatalyst FA@GRs in Example 15 of this invention;
[0041] Figure 11 This is a SEM image of the fulvic acid-green rust composite photocatalyst FA@GRs in Example 15 of this invention;
[0042] Figure 12 Raman plot of fulvic acid-green rust composite photocatalyst FA@GRs in Example 15 of this invention;
[0043] Figure 13 XRD pattern of fulvic acid-green rust composite photocatalyst FA@GRs in Example 15 of this invention;
[0044] Figure 14 These are the EPR graphs of the fulvic acid-green rust composite photocatalyst FA@GRs in Example 15 of this invention and the superoxide radical detection in blank group 2;
[0045] Figure 15 These are the EPR graphs of the fulvic acid-green rust composite photocatalyst FA@GRs in Example 15 of this invention and the singlet oxygen detection in blank group 2;
[0046] Figure 16 This is the EPR spectrum of the fulvic acid-green rust composite photocatalyst FA@GRs and the blank group for the detection of 2-hydroxyl radicals in Example 15 of this invention;
[0047] Figure 17 This is a graph showing the degradation efficiency of fulvic acid-green rust composite photocatalyst FA@GRs on bisphenol A and bisphenol F in Example 15 of this invention. Detailed Implementation
[0048] To further illustrate the methods and effects of this invention, the technical solution of this invention will be clearly and completely described below in conjunction with experiments.
[0049] Example 1: A method for preparing an organic matter-green rust composite photocatalyst, comprising the following steps:
[0050] S1. Dissolve 8.32 mmol of anhydrous FeCl3, 0.409 mmol of humic acid and 0.264 mol of sodium acetate trihydrate in a glass beaker containing 50 mL of glycerol, and stir at 80 °C for 30 min until well mixed to obtain a composite solution.
[0051] S2. Transfer the composite solution to a 100 mL polytetrafluoroethylene-lined stainless steel hydrothermal reactor, seal it, and maintain it at 200°C for 24 h.
[0052] S3. After the reactor cools to 25°C, open the reactor and pour off the liquid material on top to obtain wet powder. Take out the wet powder and wash it four times with anhydrous ethanol and ethanol solution in sequence. Then dry it in an oven at 60°C for 11 hours to obtain humic acid-green rust composite photocatalyst, denoted as HA@GRs. The ethanol solution is obtained by mixing deionized water and ethanol in a volume ratio of 1:1.
[0053] HA@GRs were used for the photocatalytic degradation of bisphenol pollutants. The method for photocatalytic degradation of bisphenol pollutants was as follows: 50 mL of bisphenol pollutants BPF and BPS were sequentially added to a reaction tube, and then 20 mg of humic acid-green rust composite photocatalyst was added to each. The tube was then irradiated with a 500W xenon lamp simulating sunlight for 10 hours to complete the photodegradation experiment. The xenon lamp wavelength was 465 nm, and the light power density was 214 mW / cm². 2 .
[0054] Example 2: Unlike Example 1, in step S1, 7.77 mmol of anhydrous FeCl3, 0.409 mmol of humic acid and 0.260 mol of sodium acetate trihydrate were dissolved in a glass beaker containing 50 mL of glycerol and stirred at 75 °C for 35 min until homogeneous to obtain a composite solution.
[0055] Example 3: Unlike Example 1, in step S1, 8.59 mmol of anhydrous FeCl3, 0.409 mmol of humic acid and 0.268 mol of sodium acetate trihydrate were dissolved in a glass beaker containing 50 mL of glycerol and stirred at 85 °C for 25 min until homogeneous to obtain a composite solution.
[0056] Example 4: Unlike Example 1, in step S2, the container is sealed and kept at 190°C for 26 hours.
[0057] Example 5: Unlike Example 1, in step S2, the container is sealed and kept at 210°C for 22 hours.
[0058] Example 6: Unlike Example 1, in step S3, the product is dried in an oven at 55°C for 12 hours.
[0059] Example 7: Unlike Example 1, in step S3, the product is dried in an oven at 65°C for 10 hours.
[0060] Example 8: Unlike Example 1, in step S3, the organic matter-green rust composite photocatalyst undergoes surface treatment before drying.
[0061] The surface treatment method is as follows: nano-Au and nano-Ag particles are alternately magnetron sputtered onto the surface of the washed organic-green rust composite photocatalyst to obtain a base film with a thickness of 8nm per layer. The sputtering range of the base film occupies 1 / 2 of the surface of the organic-green rust composite photocatalyst, and the sputtering position of each base film coincides with the previous base film. The total thickness of the base film is 4μm. Then, a composite mixture is vapor-deposited on the surface of the outermost base film using microwave plasma to obtain the outer shell layer. During magnetron sputtering, nitrogen gas is introduced at a flow rate of 28sccm for blowing, and the treatment is carried out at a temperature of 150℃ for 125s.
[0062] The particle sizes of both nano-Au and nano-Ag particles are 10-17 nm; the parameters for magnetron sputtering film formation are: substrate pressure of 3 × 10⁻⁶. -4 The film formation pressure was 0.6 Pa, the sputtering target power was 110 W, and the vapor deposition parameters were: oxygen as the deposition gas source, 1100 W as the vapor deposition temperature, 7 kPa as the deposition pressure, and 0.8 s as the gas residence time.
[0063] The composite mixture comprises, by mass percentage: 40% Al2O3 solution with a concentration of 0.8 mg / mL, 7% fluoroboron pyrrole dye, 18% surfactant, and the balance being an organic solvent; wherein the surfactant is a commercially available surfactant, sodium dodecyl sulfate is selected in this embodiment, and commercially available ethanol is selected as the organic solvent.
[0064] Example 9: Unlike Example 8, in the surface treatment method, nitrogen gas was introduced during magnetron sputtering at a flow rate of 25 sccm and treated at a temperature of 100°C for 200 s.
[0065] Example 10: Unlike Example 8, in the surface treatment method, nitrogen gas was introduced at a flow rate of 30 sccm during magnetron sputtering, and the treatment was carried out at a temperature of 200°C for 50 seconds.
[0066] Example 11: Unlike Example 8, in the surface treatment method, the particle size of both the nano-Au particles and nano-Ag particles is 2-9 nm; the parameters for magnetron sputtering film formation are: substrate pressure of 2 × 10⁻⁶. -5 The film formation pressure was 0.3 Pa, the sputtering target power was 70 W, and the vapor deposition parameters were: the deposition gas source was oxygen, the vapor deposition temperature was 1000 W, the deposition pressure was 5 kPa, and the gas residence time was 1 s.
[0067] Example 12: Unlike Example 8, in the surface treatment method, the particle size of both the nano-Au particles and nano-Ag particles is 18-25 nm; the parameters for magnetron sputtering film formation are: substrate pressure of 5 × 10⁻⁶. -4The film formation pressure was 0.8 Pa, the sputtering target power was 150 W, and the vapor deposition parameters were: the deposition gas source was oxygen, the vapor deposition temperature was 1200 W, the deposition pressure was 12 kPa, and the gas residence time was 0.5 s.
[0068] Example 13: Unlike Example 8, the composite mixture, by mass percentage, includes: 35% Al2O3 solution with a concentration of 0.5 mg / mL, 10% fluoroboron pyrrole dye, 15% surfactant, and the balance organic solvent.
[0069] Example 14: Unlike Example 8, the composite mixture, by mass percentage, includes: 45% Al2O3 solution with a concentration of 1 mg / mL, 5% fluoroboron pyrrole dye, 20% surfactant, and the balance organic solvent.
[0070] Example 15: Unlike Example 1, a method for preparing an organic matter-green rust composite photocatalyst is described. In step S1, 7.85 mmol of anhydrous FeCl3, 0.302 mmol of fulvic acid and 0.0264 mol of sodium acetate trihydrate are dissolved in a glass beaker containing 50 mL of glycerol to obtain the corresponding fulvic acid-green rust composite photocatalyst, denoted as FA@GRs.
[0071] The photocatalytic degradation of bisphenol A (BPF) pollutants using FA@GRs included the following steps: 50 mL of each BPF and BPS pollutant were sequentially placed in a reaction tube, and then 20 mg of fulvic acid-green rust composite photocatalyst was added to each. The tube was then irradiated with a 500W xenon lamp simulating sunlight for 10 hours to complete the photodegradation experiment. The xenon lamp wavelength was 465 nm, and the light power density was 214 mW / cm². 2 .
[0072] Example 16: Unlike Example 15, in step S1, 7.55 mmol of anhydrous FeCl3, 0.302 mmol of fulvic acid and 0.0261 mol of sodium acetate trihydrate are dissolved in a glass beaker containing 50 mL of glycerol.
[0073] Example 17: Unlike Example 15, in step S1, 8.15 mmol of anhydrous FeCl3, 0.302 mmol of fulvic acid and 0.0267 mol of sodium acetate trihydrate are dissolved in a glass beaker containing 50 mL of glycerol.
[0074] Experimental Example: The description of this experimental example is based on the scheme described in Example 1, and aims to illustrate the practical application effect of the present invention.
[0075] Depend on Figures 1-17It can be seen that the organic matter-green rust composite photocatalyst prepared by the present invention has superior photocatalytic performance.
[0076] Diagrammatic analysis: From Figure 1 The adsorption-desorption isotherm of the humic acid-chlorophyll composite photocatalyst exhibits a type IV isotherm with an H3 hysteresis loop, confirming the existence of a mesoporous structure in the composite catalyst. The pore size distribution is mainly concentrated in the 5-80 nm range, with an increased average pore size. This indicates that the addition of humic acid and chlorophyll improves the pore structure of the material, providing more active sites and thus enhancing its photocatalytic performance. Figure 2 It can be seen that at a wavelength of 3423.9cm -1 The peak at 1249.4 cm⁻¹ is caused by the stretching mode of a hydroxide-like layer or OH groups embedded in water molecules. -1 CO3 2- Characteristic peaks of type rust. At a wavelength of 2867.4 cm⁻¹. -1 The characteristic peak appearing at 1628.9 cm⁻¹ is attributed to the vibration of CH₃. -1 and 1123.9cm -1 The characteristic peak appearing at 826 cm⁻¹ is attributed to the stretching vibrations of C=O and CO. -1 and 676cm -1 The absorption peak of the wavelength is related to the vibration of metal-hydroxyl (M-OH) or metal-oxygen (MO) (M=Fe), indicating that the addition of humic acid makes the surface of the humic acid-green rust composite photocatalyst rich in functional groups, which can promote the reduction of iron in the catalyst and thus enhance the catalyst's degradation ability.
[0077] Depend on Figure 3 It can be seen that: at a Raman frequency shift of 427 cm -1 There is obvious green rust (CO3) 2- The characteristic peaks of the (type) further confirm that the synthesized photocatalytic material has a green rust material structure; by Figure 4 It can be seen that the humic acid-green rust composite photocatalyst exhibits a regular, plate-like, "petal-like" polymer structure with a roughened surface. This structure helps to increase the specific surface area and pore volume of the catalyst, improve its ability to adsorb pollutants, and increase the effective contact area between the catalyst and pollutants, thereby enhancing the catalyst's oxidative degradation ability. Figure 5 It can be seen that the peaks at 10.9°, 22.2°, and 33.3° of the humic acid-green rust composite photocatalyst correspond to green rust (CO3) and CO3) respectively. 2- The presence of the 003, 006, and 009 crystal planes (of type 1) indicates that the humic acid-green rust composite photocatalyst was successfully synthesized and possesses good crystallinity.
[0078] Depend on Figures 6-8It can be seen that the humic acid-green rust composite photocatalyst in Example 1, compared with the green rust catalyst in blank group 1, produces significantly more superoxide radicals, singlet oxygen radicals, and hydroxyl radicals. This result is consistent with the experimental results of photocatalytic degradation of BPA and BPF.
[0079] Depend on Figure 9 It can be seen that under xenon lamp irradiation, the humic acid-green rust composite photocatalyst of Example 1 can effectively degrade BPA and BPF. After 10 hours of photocatalytic degradation reaction, the removal rate of BPA and BPF is 80%, indicating that the humic acid-green rust composite photocatalyst of the present invention can be used as an environmentally friendly new degradation material, which can effectively remove bisphenol pollutants in organic wastewater.
[0080] Depend on Figure 10 It can be seen that at a wavelength of 3423.9cm -1 The peak at 1249.4 cm⁻¹ is caused by the stretching mode of a hydroxide-like layer or OH groups embedded in water molecules. -1 CO3 2- Characteristic peaks of type rust. At a wavelength of 1628.9 cm⁻¹. -1 and 1123.9cm -1 The characteristic peak appearing at 2867.4 cm⁻¹ is attributed to the stretching vibrations of C=O and CO. -1 The characteristic peak appearing at 826 cm⁻¹ is attributed to the vibration of CH₃. -1 and 676cm -1 The absorption peaks at the specified wavelengths are related to the vibrations of metal-hydroxyl (M-OH) or metal-oxygen (MO) (M=Fe), indicating that the addition of fulvic acid enriches the surface of the fulvic acid-green rust composite photocatalyst with functional groups, which can promote the reduction of iron in the catalyst and thus enhance its degradation ability. Figure 11 It can be seen that the morphological characteristics of the fulvic acid-green rust composite photocatalyst exhibit a regular lamellar polymer structure with a roughened surface. This structure helps to increase the specific surface area and pore volume of the catalyst, improve the catalyst's ability to adsorb pollutants, increase the effective contact area between the catalyst and pollutants, and thus enhance the catalyst's oxidative degradation ability. Figure 12 It can be seen that the Raman frequency shift is 410-427 cm. -1 There is obvious green rust (CO3) 2- The characteristic peaks of the (type) further confirm that the synthesized photocatalytic material has a green rust material structure; by Figure 13 It can be seen that the peaks appearing at 10.9°, 22.2°, and 33.3° of the fulvic acid-green rust composite photocatalyst correspond to green rust (CO3) and CO3) respectively. 2- The presence of the 003, 006, and 009 crystal planes (of type 1) indicates that the fulvic acid-green rust composite photocatalyst was successfully synthesized and possesses good crystallinity.
[0081] Depend on Figures 14-16 It can be seen that the fulvic acid-green rust composite photocatalyst of Example 15, compared with the green rust catalyst of blank group 2, produces significantly more superoxide radicals, singlet oxygen radicals, and hydroxyl radicals. This result is consistent with the experimental results of photocatalytic degradation of BPA and BPF.
[0082] Depend on Figure 17 It can be seen that under xenon lamp irradiation, the fulvic acid-green rust composite photocatalyst of Example 15 can effectively degrade BPA and BPF. After 10 hours of photocatalytic degradation reaction, the BPF removal rate is 80% and the BPA removal rate is 78%, indicating that the fulvic acid-green rust composite photocatalyst of the present invention can be used as an environmentally friendly new degradation material, which can effectively remove bisphenol pollutants in organic wastewater.
[0083] 1. Experimental Design: To elucidate the photocatalytic performance of the organic matter-green rust composite photocatalyst prepared in this invention, the following experimental group was designed:
[0084] Blank Group 1: Unlike Example 1, anhydrous FeCl3 was used alone as the photocatalyst.
[0085] Blank Group 2: Unlike Example 15, anhydrous FeCl3 was used alone as the photocatalyst.
[0086] Comparative Example 1: Unlike Example 8, the nano-Au particles and nano-Ag particles were not subjected to alternating magnetron sputtering, but were sputtered sequentially in single passes.
[0087] Comparative Example 2: Unlike Example 8, the fluoroboron pyrrole dye in the composite mixture was replaced with methylene blue, and the organic solvent was replaced with water.
[0088] Comparative Example 3: Unlike Example 8, nitrogen purging was not performed during magnetron sputtering.
[0089] 2. Relevant performance experiments: The actual performance of the present invention was compared under different experimental conditions. Specific data are shown in Table 1 and Table 2.
[0090] Table 1. Degradation performance of the organic matter-green rust composite photocatalysts prepared in Examples 1 to 7 on bisphenol pollutants.
[0091]
[0092] Conclusion: Table 1 shows that in Examples 1-7, the molar ratio of green rust, organic matter, and sodium acetate trihydrate within the scope of this application, slight variations in stirring parameters, sealing temperature and time, and differences in oven drying temperature and time had little impact on the degradation performance of the prepared organic matter-green rust composite photocatalyst for bisphenol pollutants. Figures 1-9 It can be seen that Example 1 has better photocatalytic performance than blank group 1. Considering the comprehensive data and economic factors, Example 1 is selected as the better solution among Examples 1 to 7.
[0093] Table 2. Degradation performance of organic matter-green rust composite photocatalysts prepared in Examples 1, 8-14 and Comparative Examples 1-3 on bisphenol pollutants.
[0094]
[0095] As can be seen from the data in Table 2, the organic matter-green rust composite photocatalysts obtained in Examples 8-14 showed improved degradation performance of bisphenol pollutants compared to Example 1. In Example 8, the photocatalyst achieved a catalytic efficiency of 89% within 10 hours, mainly due to the surface plasmon resonance (SPR) effect of Au and Ag nanoparticles. This effect significantly enhances the photocatalyst's light absorption in the visible light region. Alternating magnetron sputtering of Au and Ag nanoparticles creates SPR hotspots on the photocatalyst surface, thereby improving its activity. The deposition of the Al2O3 film protects the photocatalyst from environmental corrosion and provides additional photocatalytic active sites, further improving photocatalytic efficiency. Therefore, surface treatment of the organic matter-green rust composite photocatalyst before drying can further improve its stability and accelerate the photocatalytic reaction rate. However, a comparison of the data from Example 8 and Comparative Example 1 shows that Comparative Example 1 lacked the alternating film formation of metal nanoparticles (Au and Ag). The single-film formation method had limited effect on improving the stability of the photocatalyst, thus leading to a lower efficiency in the prepared organic matter-green rust composite photocatalyst. The degradation performance of the green rust composite photocatalyst for bisphenol pollutants decreased. Examples 8-14, by alternately preparing nano-Au and nano-Ag particles, formed a multifunctional composite film with high hardness, high wear resistance, and high corrosion resistance. In Control Example 2, fluoroboron pyrrole dye was replaced with methylene blue. It is evident that although the degradation performance of the organic matter-green rust composite photocatalyst prepared in Control Example 2 for bisphenol pollutants was improved compared to Example 1, it was still far lower than that of the organic matter-green rust composite photocatalysts in Examples 8-14. This is because compared to fluoroboron pyrrole... While the dye, methylene blue, may not be as stable and sensitive in optical properties as the former (as in Comparative Example 2), its improvement on the photocatalytic performance of the organic-rust composite photocatalyst is limited, although the cost of Comparative Example 2 is relatively low. Comparative Example 3, lacking the nitrogen blowing and temperature control steps during magnetron sputtering, positively impacts the interfacial properties between the gold and silver nanofilms and the photocatalyst, promoting electron transport and photogenerated carrier separation. This helps reduce the recombination probability of electrons and holes, improving photocatalytic efficiency. Furthermore, nitrogen blowing protects the photocatalyst surface, reducing oxidation or corrosion during sputtering. In addition, nitrogen can react with metal nanoparticles to form a nitride layer, further enhancing the stability of the photocatalyst. Therefore, considering all factors, Example 8 is selected as the optimal solution.
Claims
1. A method for preparing an organic matter-green rust composite photocatalyst, characterized in that, Includes the following steps: S1. Dissolve anhydrous FeCl3, organic matter, and sodium acetate trihydrate in an organic solvent, and stir at 75-85℃ for 25-35 minutes to obtain a composite solution; the organic matter is humic acid or fulvic acid. S2. Transfer the composite solution to a stainless steel hydrothermal reactor, seal it, and maintain it at 190-210℃ for 22-26 hours. S3. After the reactor cools to room temperature, open the reactor and pour off the liquid substance on the top to obtain wet powder. Take out the wet powder and wash, surface treat and dry it to obtain the organic matter-green rust composite photocatalyst. The surface treatment method is as follows: Nano-Au and nano-Ag particles are alternately magnetron sputtered onto the surface of the washed product to obtain a base film with a thickness of 5-10 nm per layer. The sputtering range of the base film occupies 1 / 4 to 3 / 4 of the surface of the organic-green rust composite photocatalyst. The total thickness of the base film is 2-5 μm. Then, a composite mixture is vapor-deposited onto the surface of the outermost base film using microwave plasma to obtain the outer shell layer. The nano-Au and nano-Ag particles have a particle size of 2-25 nm. The magnetron sputtering parameters are: substrate pressure of 2 × 10⁻⁶. -5 -5×10 -4 The film formation pressure is 0.3-0.8 Pa, the sputtering target power is 70-150 W; the vapor deposition parameters are: the deposition gas source is oxygen, the vapor deposition temperature is 1000-1200 W, the deposition pressure is 5-12 kPa, and the gas residence time is 0.5-1 s. The composite mixture comprises, by mass percentage: 35-45% Al2O3 solution with a concentration of 0.5-1 mg / mL, 5-10% fluoroboron pyrrole dye, 15-20% surfactant, and the balance being organic solvent.
2. The preparation method of the organic matter-green rust composite photocatalyst as described in claim 1, characterized in that, In step S1, the molar ratio of anhydrous FeCl3, humic acid and sodium acetate trihydrate is 19-21:1:63.5-65.5, and the molar ratio of anhydrous FeCl3, fulvic acid and sodium acetate trihydrate is 25-27:1:86.4-88.
4.
3. The preparation method of the organic matter-green rust composite photocatalyst as described in claim 1, characterized in that, In step S1, the organic solvent is glycerol.
4. The preparation method of the organic matter-green rust composite photocatalyst as described in claim 1, characterized in that, In step S3, the washing method is as follows: washing with anhydrous ethanol and ethanol solution 3-5 times in sequence; the ethanol solution is obtained by mixing deionized water and ethanol in a volume ratio of 1:
1.
5. The preparation method of the organic matter-green rust composite photocatalyst as described in claim 1, characterized in that, In step S3, the drying method is as follows: drying in an oven at 55-65℃ for 10-12 hours.
6. The preparation method of the organic matter-green rust composite photocatalyst as described in claim 1, characterized in that, In magnetron sputtering, nitrogen gas is introduced at a flow rate of 25-30 sccm for blowing, and the process is carried out at a temperature of 100-200℃ for 50-200 seconds.
7. The application of an organic matter-green rust-stabilized photocatalyst, based on the organic matter-green rust-stabilized photocatalyst prepared by the method according to any one of claims 1-6, characterized in that, The catalyst was used for the photocatalytic degradation of bisphenol pollutants.
8. The application of the organic matter-green rust-stabilized photocatalyst as described in claim 7, characterized in that, The method for photocatalytic degradation of bisphenol pollutants is as follows: 45-55 mL of bisphenol pollutants (BPF and BPA) are sequentially added to a reaction tube, followed by the addition of 18-22 mg of an organic matter-green rust composite photocatalyst. The tube is then irradiated with a 480-520 W xenon lamp simulating solar conditions for 8-12 hours to complete the photodegradation experiment. The xenon lamp wavelength is 350-780 nm, and the light power density is 214 mW / cm². 2 .