Molding method of powder high-temperature high-entropy alloy blade

Through the method of combining ceramic cover with thermal isostatic pressing, the matching problem of high-temperature high-entropy alloy components powder and ceramic cover is solved, and the near-net forming of powder high-temperature high-entropy alloy blades is achieved, dimensional accuracy and performance are optimized, and cost is reduced .

CN118875280APending Publication Date: 2024-11-01AVIC BEIJING INST OF AERONAUTICAL MATERIALS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410791418.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-19
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

At this stage, the physical characteristics of the new high-temperature high-entropy alloy composition powder, the strength of the ceramic cover, the temperature transfer and pressure transfer characteristics, and the powder shrinkage law under thermal coupling are unclear, which affects the thermal isostatic pressure near-net forming of the new high-temperature high-entropy alloy powder. Control of dimensional accuracy during the process.

Method used

Using the method of ceramic cover combined with thermal isostatic pressing, a reasonable thermal isostatic pressing process is formulated by reasonably mixing the slurry components of the surface layer and back layer to achieve near-net forming of powder high-temperature high-entropy alloy blades, reducing processing volume and reducing cost.

Benefits of technology

It has achieved excellent performance of powder high-temperature and high-entropy alloy blades, with small structure, uniform composition, good internal and external metallurgy quality, high dimensional accuracy, excellent physical and chemical performance, reducing processing and raw material costs and avoiding the shortcomings of traditional forming methods.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a powder high-temperature high-entropy alloy blade forming method which comprises the following steps: S1) preparing surface layer slurry on the surface of a blade wax mold, preparing alumina sand or silica sand on the surface, and drying to obtain a shell surface layer; s2) preparing back layer slurry on the surface of the shell surface layer, preparing back layer refractory material sand on the surface, reinforcing by adopting a ceramic net, and drying to obtain a ceramic shell; s3) the ceramic shell is dewaxed and then roasted, and an initial shell is obtained; and S4) packaging the high-temperature high-entropy alloy powder in the initial shell, then carrying out hot isostatic pressing, and finally removing the surface shell to obtain the powder high-temperature high-entropy alloy blade. According to the forming method for the excellent powder high-entropy alloy blade, by reasonably adjusting the proportion of surface layer and back layer component slurry and formulating a reasonable hot isostatic pressing process formulating method, the excellent forming method for the powder high-entropy alloy blade is obtained, and the development requirement of a future new generation of high-temperature aero-engine blade is met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of powder alloy forming, and in particular to a forming method of a powder high-temperature high-entropy alloy blade. Background Art

[0002] High entropy alloy is a new type of alloy material with application potential developed in recent years. It is of great significance for the development of high-temperature structural parts of the new generation of high thrust-to-weight ratio aircraft engines.

[0003] The design concept of high entropy alloy with equal atomic ratio and near equal atomic ratio makes it possible to show excellent organizational stability, specific strength and toughness in the medium and high temperature field (700℃~900℃). Powder metallurgy hot isostatic pressing technology can achieve near net forming of materials. Powder components have the characteristics of fine organization, uniform composition, good internal and external metallurgical quality, high dimensional accuracy, excellent physical and chemical properties, etc., which can avoid the shortcomings of traditional forming processes.

[0004] However, at present, the physical properties of the new high-temperature high-entropy alloy component powder, the strength of the ceramic sheath, the temperature and pressure transfer characteristics, and the shrinkage law of the powder under thermal-mechanical coupling are unclear, which will affect the control of dimensional accuracy during the hot isostatic pressing near-net forming process of the new high-temperature high-entropy alloy powder. Summary of the invention

[0005] The technical problem solved by the present invention is to provide a forming method for powder high-temperature high-entropy alloy blades, which can directly achieve near-net forming of powder high-temperature high-entropy alloy blades, reduce the processing amount of the blades, and the blades prepared by the present application have excellent performance.

[0006] In view of this, the present application provides a method for forming a powder high-temperature high-entropy alloy blade, comprising the following steps:

[0007] S1) preparing a surface layer slurry on the surface of a blade wax mold, and then preparing aluminum oxide sand or silicon oxide sand on the surface, and drying to obtain a mold shell surface layer;

[0008] The surface layer slurry includes one of aluminum oxide and silicon oxide, and a liquid binder;

[0009] S2) preparing a back layer slurry on the surface of the shell surface layer, and then preparing a back layer refractory sand on the surface, and using a ceramic mesh to reinforce it, and after drying to obtain a ceramic shell; the back layer slurry includes a refractory material and a liquid binder;

[0010] S3) dewaxing and calcining the ceramic shell to obtain an initial shell;

[0011] S4) placing the high temperature high entropy alloy powder in an initial mold shell for packaging, then performing hot isostatic pressing, and finally removing the surface mold shell to obtain a powder high temperature high entropy alloy blade.

[0012] Preferably, the composition of the high temperature high entropy alloy powder includes Ni-Co-Fe-Cr-Al-Ti, the particle size of the high temperature high entropy alloy powder is 30-120 μm, and the tap density is 5.0-5.5 g / cm 3 .

[0013] Preferably, in step S1), the powder-liquid weight ratio of the surface layer slurry is 1.3:1 to 3:1, the viscosity is 5 to 30s, and the liquid binder is silica sol; the particle size of one of the aluminum oxide and silicon oxide is independently 200 to 325 mesh, the particle size of the aluminum oxide sand or silicon oxide sand is 160 to 250 mesh, and the number of layers of the mold shell surface layer is 2 to 3 layers.

[0014] Preferably, in step S2), the refractory material is bauxite, the liquid binder is silica sol, the powder-liquid weight ratio of the back layer slurry is 1:1 to 1:3, the viscosity is 5 to 10s, and the number of back layers of the ceramic shell is 4 to 5.

[0015] Preferably, the ceramic mesh is a SiC fiber mesh or a C fiber mesh; the steps of reinforcing the ceramic mesh are specifically as follows:

[0016] After preparing the second layer of back refractory sand, use ceramic mesh to reinforce it, dry it, and then prepare another back refractory sand, and then use ceramic mesh to reinforce it, dry it, and repeat this process several times until the last layer of ceramic mesh is reinforced and dried.

[0017] Preferably, the dewaxing temperature is 500-800°C, and the time is 1-2 hours; the calcining temperature is 1000-1500°C, and the time is 2-6 hours.

[0018] Preferably, in step S3), after the calcination, the step further comprises:

[0019] The fired shell was cleaned with butanone and then subjected to endoscopic inspection.

[0020] Preferably, the hot isostatic pressing is performed at a temperature of 1100 to 1300° C., a pressure of 140 to 170 MPa, and a time of 2 to 5 hours.

[0021] Preferably, the method for removing the surface shell is specifically as follows:

[0022] Mechanical water is first used for cleaning, and then chemical alkali boiling is used to remove the residual shell material, and the reagent for the alkali boiling is sodium hydroxide.

[0023] Preferably, the wax model is prepared by a 3D printing method.

[0024] The present application provides a forming method for a powder high-temperature high-entropy alloy blade, which first prepares a surface layer slurry on the surface of a blade wax mold, then prepares alumina sand or silica sand on the surface to obtain a shell surface layer, then prepares a back layer slurry on the surface of the shell surface layer, and then prepares refractory sand on the surface to obtain a ceramic shell, then uses a ceramic mesh to fix the ceramic shell, dewaxes and then roasts to obtain an initial shell; finally, the high-temperature high-entropy alloy powder is placed in the initial shell for packaging, and the surface shell is taken out after hot isostatic pressing to obtain a powder high-temperature high-entropy alloy blade; the forming method for a powder high-temperature high-entropy alloy blade provided by the present application adopts a ceramic sheath combined with hot isostatic pressing to prepare a powder high-temperature high-entropy alloy blade, which can reduce the sheath preparation cost, and can ensure that the blade has the characteristics of fine structure, uniform composition, good internal and external metallurgical quality, high dimensional accuracy, excellent physical and chemical properties, etc.; compared with blades prepared by forging methods, the present invention can directly achieve near-net forming of powder blades, reduce blade processing volume, reduce processing costs and raw material costs, and the blades prepared by the present application have excellent performance. DETAILED DESCRIPTION

[0025] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.

[0026] In view of the fact that in the prior art forming method of powder high-temperature high-entropy alloy blades, the matching of the physical properties of high-temperature high-entropy alloy powder and the ceramic sheath is not well studied, which will eventually affect the problem of the near-net-shape dimensional accuracy of the hot isostatic pressing of the powder high-temperature high-entropy alloy, the present application provides a forming method of powder high-temperature high-entropy alloy blades, which obtains powder high-temperature high-entropy alloy blades with excellent performance through the matching of the surface layer slurry, the back layer slurry, the ceramic mesh, and the hot isostatic pressing, and also realizes the near-net-shape forming of the powder high-temperature high-entropy alloy blades, reduces the processing amount of the blades, and reduces the processing cost and the cost of raw materials. Specifically, the present application provides a forming method of powder high-temperature high-entropy alloy blades, comprising the following steps:

[0027] S1) preparing a surface layer slurry on the surface of a blade wax mold, and then preparing aluminum oxide sand or silicon oxide sand on the surface, and drying to obtain a mold shell surface layer;

[0028] The surface layer slurry includes one of aluminum oxide and silicon oxide, a liquid binder and water;

[0029] S2) preparing a back layer slurry on the surface of the mold shell surface layer, and then preparing a back layer refractory sand on the surface, and drying to obtain a ceramic mold shell;

[0030] The backing slurry comprises a refractory material and a liquid binder;

[0031] S3) fixing the ceramic shell with a ceramic mesh, dewaxing and then firing to obtain an initial shell;

[0032] S4) placing the high temperature high entropy alloy powder in an initial mold shell for packaging, then performing hot isostatic pressing, and finally removing the surface mold shell to obtain a powder high temperature high entropy alloy blade.

[0033] In the molding method of powder high-temperature high-entropy alloy blades, the present application first prepares a blade wax mold, and the blade wax mold is preferably prepared by a 3D printing method, and the wax material of the wax mold is preferably blue high-strength wax.

[0034] According to the present invention, the surface layer of the ceramic sheath is prepared, specifically: one of aluminum oxide and silicon oxide is mixed with a liquid binder to obtain a surface layer slurry, the surface layer slurry is prepared on the surface of the blade wax mold, and then aluminum oxide sand or silicon oxide sand is prepared on the surface, and the surface layer of the ceramic sheath, i.e., the shell surface layer, is obtained after drying. In the above process, the liquid binder is silica sol, the particle size of the aluminum oxide or silicon oxide is 200-325 meshes, specifically, the particle size of the aluminum oxide or silicon oxide is 250-300 meshes, the particle size of the aluminum oxide sand or silicon oxide sand is 160-250 meshes, specifically, the particle size of the aluminum oxide sand or silicon oxide sand is 170-220 meshes; the mesh number of the particle size of the aluminum oxide or silicon oxide is greater than the mesh number of the aluminum oxide sand or silicon oxide sand. The powder-liquid weight ratio of the surface layer slurry is 1.3:1 to 3:1, more specifically, the powder-liquid weight ratio is 1.3:1, 1.4:1, 1.5:1, 1.6:1, 1.7:1, 1.8:1, 1.9:1, 1.9:1, 2.0:1, 2.1:1, 2.2:1, 2.3:1, 2.4:1, 2.5:1, 2.6:1, 2.7:1, 2.8:1, 2.9:1 or 3.0:1. The viscosity of the surface layer slurry is 5 to 30s, specifically, the viscosity of the surface layer slurry is 7 to 25s, more specifically, the viscosity of the surface layer slurry is 10 to 20s. The surface layer slurry may also include a defoamer and / or water, and the specific selection of the defoamer is in accordance with the selection known to those skilled in the art, and there is no particular limitation in this application. The above-mentioned preparation means can be carried out by coating. The number of the mold shell surface layer is 2 to 3 layers, that is, 2 to 3 layers, more specifically 2 layers, of the mold shell surface layer are prepared according to the above method.

[0035] The present application then prepares a back layer slurry on the surface of the mold shell surface layer, and then prepares a back layer refractory sand on the surface, and uses a ceramic mesh for reinforcement, and obtains a ceramic mold shell after drying; the above-mentioned preparation means can be used in a manner well known to technical personnel in the field, such as coating. The refractory material is bauxite, the liquid binder is aluminum sol, and the powder-liquid ratio of the back layer slurry is 1:1 to 1:3. Specifically, the powder-liquid ratio of the back layer slurry is 1:1, 1:1.2, 1:1.4, 1:1.5, 1:1.8, 1:2, 1:2.2, 1:2.3, 1:2.5, 1:2.6, 1:2.8, 1:2.9 or 1:3. The viscosity of the back layer slurry is 5 to 30s, specifically, the viscosity of the back layer slurry is 6 to 26s, more specifically, the viscosity of the back layer slurry is 10 to 22s, and more specifically, the viscosity of the back layer slurry is 13 to 18s. The refractory sand is bauxite sand. The particle size of the bauxite is 160-200 mesh, and the particle size of the bauxite sand is 30-80 mesh. More specifically, the particle size of the bauxite is 160 mesh, 170 mesh, 180 mesh, 190 mesh or 200 mesh, and the particle size of the bauxite sand is 30 mesh, 40 mesh, 50 mesh, 60 mesh, 70 mesh or 80 mesh. According to the above method, 4-5 back layers, specifically 4 layers, are prepared on the mold shell surface layer.

[0036] In the above steps of preparing the surface layer and the back layer, the powder-to-liquid weight ratio of the slurry will affect the quality of the ceramic sheath, and the quality of the ceramic sheath will affect the powder metallurgy quality, dimensional accuracy, the presence of cracks, and whether it can be completely formed. The larger the powder-to-liquid weight ratio, the thicker the coating, resulting in poor air permeability on the surface of the ceramic sheath, which will cause pore defects in the powder blades; on the other hand, too thick will cause the sand to float on the surface, which will not have a good strengthening effect, reducing the strength of the ceramic sheath. If the strength of the ceramic sheath is not enough, the ceramic sheath will deform during the hot isostatic pressing process, and it will crack severely. The deformation of the ceramic sheath will cause the powder blades to deform. The powder blades will shrink under high temperature and high pressure to complete the densification process. The more layers of the surface layer and the back layer, the stronger the strength of the ceramic sheath. If the strength of the ceramic sheath is too high, the ceramic sheath will decrease its ability to deform as the powder blades shrink, resulting in microcracks or tearing in the powder blades. In the present application, the number of layers of the shell surface layer will also affect the quality of the blade. The surface layer is used to prevent the powder high-temperature high-entropy alloy from reacting with the ceramic shell material under high temperature and high pressure, resulting in the final ceramic sheath being difficult to remove, thereby affecting the progress of the powder high-temperature high-entropy alloy blade. The number of back layers of the ceramic shell directly affects the strength of the ceramic sheath and the yieldability of the sheath. The more layers, the higher the sheath strength, the thicker the ceramic sheath, and the worse the yieldability.

[0037] In the above-mentioned ceramic mesh reinforcement process, specifically: after the back layer slurry is prepared, several layers of back layer refractory material sand layer can be prepared on the surface of the back layer slurry layer, after preparing several layers of back layer refractory material sand layer, ceramic mesh is used on its surface for reinforcement, dried, and then a back layer refractory sand layer is prepared, and then ceramic mesh is used for reinforcement, dried, and the process is repeated several times until the last layer of ceramic mesh reinforcement is dried. Taking the preparation of the second layer of back layer slurry layer and starting to reinforce the ceramic mesh as an example, it is more specifically: after the back layer slurry is prepared on the surface of the mold shell surface layer, the first layer of back layer refractory material sand layer is prepared on the surface of the back layer slurry layer, dried, the second layer of back layer refractory material sand layer is prepared, and then ceramic mesh is used for reinforcement on the surface, dried, the third layer of back layer refractory material sand layer is prepared, and then ceramic mesh is used for reinforcement on the surface, dried, the fourth layer of back layer refractory material sand layer is prepared, and then ceramic mesh is used for reinforcement on the surface, dried, and the above steps are repeated until the last layer. The ceramic mesh may be Si fiber or C fiber. More specifically, the Si fiber is a woven two-dimensional fiber cloth, and the C fiber is a woven two-dimensional fiber cloth. The ceramic mesh may be reinforced starting from the second layer of the back layer until the last back layer.

[0038] The present application then dewaxes the ceramic shell and then bakes it to obtain the initial shell; in the present application, the dewaxing temperature is 500-800°C, and the time is 1-2h, specifically, the dewaxing temperature is 520-760°C, more specifically, the dewaxing temperature is 550-720°C, more specifically, the dewaxing temperature is 580-680°C; the baking temperature is 1000-1500°C, and the time is 2-6h, specifically, the baking temperature is 1100-1400°C, specifically, the baking temperature is 1120-1350°C, more specifically, the baking temperature is 1180-1250°C; the baking time is 2.5-5.5h, specifically, the baking time is 3-5h, more specifically, the baking time is 3.5-4.5h.

[0039] According to the present invention, after calcination, the calcined ceramic sheath can be cleaned and inspected by endoscope; the cleaning can be specifically carried out by butanone cleaning to remove oil stains and impurities, and the inspection is to determine whether there are cracks or bulging on the surface of the ceramic sheath, and it can be used after passing the inspection.

[0040] The present application then puts the powdered high-temperature high-entropy alloy into the above-mentioned package for packaging and degassing. The composition of the high-temperature high-entropy alloy powder includes Ni-Co-Fe-Cr-Al-Ti, and the D50 particle size of the high-temperature high-entropy alloy powder is 30-120 μm, and the tap density is 5.0-5.5 g / cm 3 Specifically, the composition of the high temperature high entropy alloy powder includes Ni-Co 23~25 -Fe 5~8 -Cr8~10 -Al 7~9 -Ti 3~6 (at%); the D50 particle size is 50 to 100 μm, more specifically, the D50 particle size is 60 to 90 μm, and the tap density is 5.0 g / cm 3 , 5.1g / cm 3 , 5.2g / cm 3 , 5.3g / cm 3 , 5.4g / cm 3 or 5.5g / cm 3 The powder high temperature high entropy alloy is packaged and then hot isostatically pressed, the temperature of the hot isostatic pressing is 1100-1300°C, the pressure is 140-170MPa, and the time is 2-5h; more specifically, the temperature of the hot isostatic pressing is 1100°C, 1200°C, 1300°C, the pressure is 140MPa, 150MPa, 160MPa, 170MPa, and the time is 2h, 3h, 4h or 5h.

[0041] The present application finally removes the surface shell to obtain a powder high-temperature high-entropy alloy blade, and the removal method is specifically: first mechanical water removal, and then chemical alkali boiling to remove the residual shell material, and the alkali boiling reagent is sodium hydroxide.

[0042] The present invention discloses a forming method of a powder high-temperature high-entropy alloy blade, and the present invention relates to a new type of high-temperature high-entropy alloy, which exhibits relatively excellent organizational stability, specific strength, and toughness in the medium and high temperature field (700°C to 900°C). At present, the physical properties of the new type of high-temperature high-entropy alloy component powder, the strength of the ceramic sheath, the temperature and pressure transfer characteristics, and the shrinkage law of the powder under the action of thermomechanical coupling are unclear, which will affect the control of dimensional accuracy during the hot isostatic pressing near-net forming process of the new type of powder high-entropy alloy. The present invention reasonably adjusts the slurry ratio of the surface layer and back layer components of the ceramic sheath, formulates a reasonable hot isostatic pressing process formulation method, and obtains an excellent forming method of a powder high-entropy alloy blade to meet the research and development needs of a new generation of high-temperature aero-engine blades in the future.

[0043] Compared with the existing powder forming technology, the present invention adopts a ceramic sheath hot isostatic pressing method to prepare high-temperature high-entropy alloy blades. Compared with metal sheaths, the sheath preparation cost can be reduced, and the powder components prepared by this method have the characteristics of fine structure, uniform composition, good internal and external metallurgical quality, high dimensional accuracy, excellent physical and chemical properties, etc., which can avoid the shortcomings of blades formed by traditional casting methods; compared with blades prepared by forging methods, the present invention can directly achieve near-net forming of powder components, reduce component processing volume, reduce processing costs and raw material costs, and the powder components disclosed in the present invention have excellent performance, which is equivalent to the performance of forged blades.

[0044] In order to further understand the present invention, the forming method of the powder high-temperature high-entropy alloy blade provided by the present invention is described in detail below in combination with the embodiments. The protection scope of the present invention is not limited by the following embodiments.

[0045] Embodiment 1 The forming method of powder high temperature high entropy alloy blades, the specific steps are as follows:

[0046] (1) The nominal alloy composition is Ni-Co 23~25 -Fe 5~8 -Cr 8~10 -Al 7~9 -Ti 3~6 (at%) series of powder high temperature high entropy alloy blades, the average particle size D50 of the powder is 80μm, and the tap density is 5.2g / cm 3 ; The minimum wall thickness of the blade is 1.2mm, the blade length is 95mm, and the torsion angle is 18°;

[0047] (2) Preparation of blade wax model: The wax model is prepared by 3D printing method, blue high-strength wax is used as the wax material, and the wax model is roughened;

[0048] (3) Preparation of ceramic jacket surface layer: Alumina and silica sol are mixed with a powder-liquid weight ratio of 1.3:1, and the slurry viscosity is controlled at 8s to obtain a surface coating, which is applied to the wax mold after roughening treatment, and then coated with alumina sand. After drying, a shell surface layer is obtained. Two layers of surface layer are prepared according to the above method; the particle size of the alumina sand is 200 mesh, and the particle size of the alumina sand is 160 mesh;

[0049] (4) Preparation of ceramic sheath back layer: bauxite powder and silica sol are mixed at a powder-liquid weight ratio of 1:1, stirred for 2 hours, and the slurry viscosity is controlled at 5-6 seconds to prepare the back layer slurry, which is applied to the shell surface layer, and then coated with back layer bauxite sand, and then slurried and dried. Four back layers are prepared according to the above method, with the particle size of bauxite powder being 160 mesh and the particle size of bauxite sand being 40 mesh;

[0050] (5) Ceramic sheath reinforcement layer protection: SiC ceramic mesh is used to fix the ceramic sheath, in which SiC fiber is a woven two-dimensional fiber cloth, and reinforcement starts from the back 2 layer until the last back layer;

[0051] (6) Firing after dewaxing of the ceramic sheath: dewaxing temperature 700°C, dewaxing time 2h, calcining temperature 1100°C, calcining time 3h;

[0052] (7) Ceramic sleeve cleaning: Use butanone to clean the wax mold to remove oil and impurities;

[0053] (8) Ceramic shell inspection: Use an endoscope to inspect the ceramic shell to see if there are cracks or bulges on the shell surface. The shell can only be used after the quality inspection is qualified.

[0054] (9) Powder packaging and degassing: high-temperature high-entropy alloy powders of different compositions are loaded into the mold shell described in step (7) for packaging and degassing;

[0055] (10) Hot isostatic pressing: Place the packaged shell into a hot isostatic pressing furnace at a hot isostatic pressing temperature of 1200°C, a pressure of 150 MPa, and a time of 2.5 h;

[0056] (11) Removal of ceramic sheath: First, mechanical water cleaning is used to clean the shell, and then chemical alkali boiling is used to remove the residual shell material. The alkali boiling liquid is sodium hydroxide;

[0057] (12) Powder blade inspection: The micro cracks on the blade surface are detected by fluorescence detection method, and then it is placed in ultrasonic testing equipment and combined with X-ray detection to evaluate its internal metallurgical quality. Finally, it is placed on a blue light scanner platform for dimensional contour scanning.

[0058] The results show that the powder high-temperature high-entropy alloy blade is fully formed, and the strength of the ceramic sheath is 5.2MPa. The ceramic sheath does not show any deformation, cracking or bulging. The minimum wall thickness of the powder blade can be controlled at ±0.2mm, there are no microcracks on the surface, and there are no metallurgical defects such as pores and inclusions inside. The grains are fine, with an average grain size of 56μm, which can meet the blade size accuracy and internal and external metallurgical quality requirements.

[0059] Embodiment 2 The forming method of powder high temperature high entropy alloy blade, the specific steps are as follows:

[0060] (1) The nominal alloy composition is Ni-Co 23~25 -Fe 5~8 -Cr 8~10 -Al 7~9 -Ti 3~6 (at%) series of powder high temperature high entropy alloy blades, the average particle size D50 of the powder is 95μm, and the tap density is 5.33g / cm 3 ; The minimum wall thickness of the blade is 1.5mm, the blade length is 105mm, and the torsion angle is 10°;

[0061] (2) Preparation of blade wax model: The wax model is prepared by 3D printing method, blue high-strength wax is used as the wax material, and the wax model is roughened;

[0062] (3) Preparation of ceramic jacket surface layer: Alumina and silica sol are mixed with a powder-liquid weight ratio of 1.5:1, and the slurry viscosity is controlled at 10s. The surface layer coating is applied to the wax mold after roughening treatment, and then alumina sand is applied. After drying, the shell surface layer is obtained. Two layers of surface layer are prepared according to the above method, and the particle size of alumina is 260 mesh and the particle size of alumina sand is 200 mesh;

[0063] (4) Preparation of ceramic sheath back layer: bauxite powder and silica sol were mixed with a powder-liquid weight ratio of 1:2.5, stirred for 2.5 hours, and the slurry viscosity was controlled at 4-5 seconds to prepare the back layer slurry. The back layer slurry was coated on the surface layer of the mold shell, and then the back layer bauxite sand was coated. The particle size of the bauxite powder was 180 mesh, and the particle size of the bauxite sand was 60 mesh. Then, the slurry was bonded and dried. Four layers of the back layer were prepared according to the above method;

[0064] (5) Ceramic sheath reinforcement layer protection: C fiber mesh is used to fix the ceramic sheath, where C fiber is a woven two-dimensional fiber cloth, and reinforcement starts from the back 2 layer until the last back layer;

[0065] (6) Calcination after dewaxing of the ceramic sheath: dewaxing temperature 680°C, dewaxing time 2h, calcination temperature 1120°C, calcination time 3h;

[0066] (7) Ceramic sleeve cleaning: Use butanone to clean the wax mold to remove oil and impurities;

[0067] (8) Ceramic shell inspection: Use an endoscope to inspect the ceramic shell to see if there are cracks or bulges on the shell surface. The shell can only be used after the quality inspection is qualified.

[0068] (9) Powder packaging and degassing: high-temperature high-entropy alloy powders of different compositions are loaded into the mold shell described in step (7) for packaging and degassing;

[0069] (10) Hot isostatic pressing: Place the packaged shell into a hot isostatic pressing furnace at a hot isostatic pressing temperature of 1230°C, a pressure of 140 MPa, and a time of 3 h;

[0070] (11) Removal of ceramic sheath: First, mechanical water cleaning is used to clean the shell, and then chemical alkali boiling is used to remove the residual shell material. The alkali boiling liquid is sodium hydroxide;

[0071] (12) Powder blade inspection: The micro cracks on the blade surface are detected by fluorescence detection method, and then it is placed in ultrasonic testing equipment and combined with X-ray detection to evaluate its internal metallurgical quality. Finally, it is placed on a blue light scanner platform for dimensional contour scanning.

[0072] The results show that the powder high-temperature high-entropy alloy blade is fully formed, and the three-point bending strength of the ceramic sheath is 6MPa, and the ceramic sheath has no deformation, cracking or bulging; the minimum wall thickness of the powder blade can be controlled at ±0.1mm, there are no microcracks on the surface, and there are no metallurgical defects such as pores and inclusions inside, and the average grain size is 63μm, which can meet the blade size accuracy and internal and external metallurgical quality requirements.

[0073] Comparative Example 1 is a method for forming a powder high-temperature high-entropy alloy blade. The difference is that the viscosity of the surface coating slurry is changed, but the number of layers remains unchanged. The specific steps are as follows:

[0074] (1) The nominal alloy composition is Ni-Co 23~25 -Fe 5~8 -Cr 8~10 -Al 7~9 -Ti 3~6 (at%) powder high temperature high entropy alloy blade, the average particle size D50 of the powder is 95μm, and the tap density is 5.33g / cm 3 ; The minimum wall thickness of the blade is 1.5mm, the blade length is 105mm, and the torsion angle is 10°;

[0075] (2) Preparation of blade wax model: The wax model is prepared by 3D printing method, blue high-strength wax is used as the wax material, and the wax model is roughened;

[0076] (3) Preparation of ceramic jacket surface layer: Alumina and silica sol were mixed with a powder-liquid weight ratio of 4:1 and a slurry viscosity of 17s. The surface layer coating was applied to the wax mold after roughening treatment, and then alumina sand was applied. After drying, the shell surface layer was obtained. Two layers of surface layer were prepared according to the above method. The alumina particle size was 260 mesh and the alumina sand particle size was 200 mesh.

[0077] (4) Preparation of ceramic sheath back layer: bauxite powder and silica sol were mixed at a powder-liquid weight ratio of 1:2.5, stirred for 2.5 hours, and the slurry viscosity was controlled at 4-5 seconds to prepare the back layer slurry. The back layer slurry was coated on the surface layer of the mold shell, and then coated with the back layer of bauxite sand, and then slurried and dried. Four back layers were prepared according to the above method. The particle size of the bauxite powder was 180 mesh, and the particle size of the bauxite sand was 60 mesh.

[0078] (5) Ceramic sheath reinforcement layer protection: C fiber mesh is used to fix the ceramic sheath, where C fiber is a woven two-dimensional fiber cloth, and reinforcement starts from the back 2 layer until the last back layer;

[0079] (6) Calcination after dewaxing of the ceramic sheath: dewaxing temperature 680°C, dewaxing time 2h, calcination temperature 1120°C, calcination time 3h;

[0080] (7) Ceramic sleeve cleaning: Use butanone to clean the wax mold to remove oil and impurities;

[0081] (8) Ceramic shell inspection: Use an endoscope to inspect the ceramic shell to see if there are cracks or bulges on the shell surface. The shell can only be used after the quality inspection is qualified.

[0082] (9) Powder packaging and degassing: high-temperature high-entropy alloy powders of different compositions are loaded into the mold shell described in step (7) for packaging and degassing;

[0083] (10) Hot isostatic pressing: Place the packaged shell into a hot isostatic pressing furnace at a hot isostatic pressing temperature of 1230°C, a pressure of 140 MPa, and a time of 3 h;

[0084] (11) Removal of ceramic sheath: First, mechanical water cleaning is used to clean the shell, and then chemical alkali boiling is used to remove the residual shell material. The alkali boiling liquid is sodium hydroxide;

[0085] (12) Powder blade inspection: The micro cracks on the blade surface are detected by fluorescence detection method, and then it is placed in ultrasonic testing equipment and combined with X-ray detection to evaluate its internal metallurgical quality. Finally, it is placed on a blue light scanner platform for dimensional contour scanning.

[0086] The results show that the powder high-temperature high-entropy alloy blade is fully formed, and the three-point bending strength of the ceramic sheath is 6MPa, and the ceramic sheath does not show deformation, cracking or bulging; the minimum wall thickness of the powder blade can be controlled at ±0.1mm, and its average grain size is 63μm, with no microcracks on the surface, which can meet the blade size accuracy, but there are a small amount of pores and mixed metallurgical defects inside the blade, which does not meet the internal metallurgical quality requirements of powder products.

[0087] Comparative Example 2 is a method for forming a powder high-temperature high-entropy alloy blade, the difference being that the number of backing layers is changed, and the specific steps are as follows:

[0088] (1) The nominal alloy composition is Ni-Co 23~25 -Fe 5~8 -Cr 8~10 -Al 7~9 -Ti 3~6 (at%) powder high temperature high entropy alloy blade, the average particle size D50 of the powder is 80μm, and the tap density is 5.2g / cm 3 ; The minimum wall thickness of the blade is 1.2mm, the blade length is 95mm, and the torsion angle is 18°;

[0089] (2) Preparation of blade wax model: The wax model is prepared by 3D printing method, blue high-strength wax is used as the wax material, and the wax model is roughened;

[0090] (3) Preparation of ceramic jacket surface layer: Alumina and silica sol are mixed with a powder-liquid weight ratio of 1.3:1, and the slurry viscosity is controlled at 8s to obtain a surface coating, which is applied to the wax mold after roughening treatment, and then coated with alumina sand. After drying, the shell surface layer is obtained. Two layers of surface layer are prepared according to the above method, with the alumina particle size of 200 mesh and the alumina sand particle size of 160 mesh;

[0091] (4) Preparation of ceramic sheath back layer: bauxite powder and silica sol are mixed at a powder-liquid weight ratio of 1:1, stirred for 2 hours, and the slurry viscosity is controlled at 5-6 seconds to prepare the back layer slurry, which is applied to the surface layer of the mold shell, and then coated with the back layer bauxite sand, and then slurried and dried. According to the above method, 7 layers of back layer are prepared, and the particle size of bauxite powder is 160 mesh, and the particle size of bauxite sand is 40 mesh;

[0092] (5) Ceramic sheath reinforcement layer protection: SiC ceramic mesh is used to fix the ceramic sheath, in which SiC fiber is a woven two-dimensional fiber cloth, and reinforcement starts from the back 2 layer until the last back layer;

[0093] (6) Firing after dewaxing of the ceramic sheath: dewaxing temperature 700°C, dewaxing time 2h, calcining temperature 1100°C, calcining time 3h;

[0094] (7) Ceramic sleeve cleaning: Use butanone to clean the wax mold to remove oil and impurities;

[0095] (8) Ceramic shell inspection: Use an endoscope to inspect the ceramic shell to see if there are cracks or bulges on the shell surface. The shell can only be used after the quality inspection is qualified.

[0096] (9) Powder packaging and degassing: high-temperature high-entropy alloy powders of different compositions are loaded into the mold shell described in step (7) for packaging and degassing;

[0097] (10) Hot isostatic pressing: Place the packaged shell into a hot isostatic pressing furnace at a hot isostatic pressing temperature of 1200°C, a pressure of 150 MPa, and a time of 2.5 h;

[0098] (11) Removal of ceramic sheath: First, mechanical water cleaning is used to clean the shell, and then chemical alkali boiling is used to remove the residual shell material. The alkali boiling liquid is sodium hydroxide;

[0099] (12) Powder blade inspection: The micro cracks on the blade surface are detected by fluorescence detection method, and then it is placed in ultrasonic testing equipment and combined with X-ray detection to evaluate its internal metallurgical quality. Finally, it is placed on a blue light scanner platform for dimensional contour scanning.

[0100] The results show that the powder high-temperature high-entropy alloy blade is fully formed, and the strength of the ceramic sheath is 10.8MPa. The ceramic sheath does not show deformation, cracking or bulging. The minimum wall thickness of the powder blade can be controlled at ±0.2mm, but microcracks appear on the surface, but there are no metallurgical defects such as pores and inclusions inside. The grains are fine, with an average grain size of 56μm, which does not meet the requirements of blade size accuracy and surface quality.

[0101] Comparative Example 3 is a method for forming a powder high-temperature high-entropy alloy blade, the difference being that the hot isostatic pressing temperature of the ceramic sheath is changed. The specific steps are as follows:

[0102] (1) The nominal alloy composition is a powder high-temperature high-entropy alloy blade of Ni-Co-Fe-Cr-Al-Ti system, with a powder mean particle size D50 of 80 μm and a tap density of 5.2 g / cm 3 ; The minimum wall thickness of the blade is 1.2mm, the blade length is 95mm, and the torsion angle is 18°;

[0103] (2) Preparation of blade wax model: The wax model is prepared by 3D printing method, blue high-strength wax is used as the wax material, and the wax model is roughened;

[0104] (3) Preparation of ceramic jacket surface layer: Alumina and silica sol are mixed, the number of surface layers is 2, the weight ratio of powder to liquid is 1.3:1, the slurry viscosity is controlled at 8s, and the surface layer coating is obtained. The surface layer coating is applied to the wax mold after roughening treatment, and then alumina sand is applied. After drying, the shell surface layer is obtained. According to the above method, 2 layers of surface layer are prepared, the particle size of alumina is 200 mesh, and the particle size of alumina sand is 160 mesh;

[0105] (4) Preparation of ceramic sheath back layer: bauxite powder and silica sol are mixed at a powder-liquid weight ratio of 1:1, stirred for 2 hours, and the slurry viscosity is controlled at 5-6 seconds to prepare the back layer slurry, which is applied to the shell surface layer, and then coated with back layer bauxite sand, and then slurried and dried. Four back layers are prepared according to the above method, with the particle size of bauxite powder being 160 mesh and the particle size of bauxite sand being 40 mesh;

[0106] (5) Ceramic sheath reinforcement layer protection: SiC ceramic mesh is used to fix the ceramic sheath, in which SiC fiber is a woven two-dimensional fiber cloth, and reinforcement starts from the back 2 layer until the last back layer;

[0107] (6) Firing after dewaxing of the ceramic sheath: dewaxing temperature 700°C, dewaxing time 2h, calcining temperature 1100°C, calcining time 3h;

[0108] (7) Ceramic sleeve cleaning: Use butanone to clean the wax mold to remove oil and impurities;

[0109] (8) Ceramic shell inspection: Use an endoscope to inspect the ceramic shell to see if there are cracks or bulges on the shell surface. The shell can only be used after the quality inspection is qualified.

[0110] (9) Powder packaging and degassing: high-temperature high-entropy alloy powders of different compositions are loaded into the mold shell described in step (7) for packaging and degassing;

[0111] (10) Hot isostatic pressing: Place the packaged shell into a hot isostatic pressing furnace at a temperature of 1000°C, a pressure of 150 MPa, and a time of 2.5 h;

[0112] (11) Removal of ceramic sheath: First, mechanical water cleaning is used to remove the shell, and then chemical alkali boiling is used to remove the residual shell material. The alkali boiling liquid is sodium hydroxide.

[0113] (12) Powder blade inspection: The micro cracks on the blade surface are detected by fluorescence detection method, and then it is placed in ultrasonic testing equipment and combined with X-ray detection to evaluate its internal metallurgical quality. Finally, it is placed on a blue light scanner platform for dimensional contour scanning.

[0114] The results show that the powder high-temperature high-entropy alloy blade is fully formed, and the strength of the ceramic sheath is 5.2MPa. The ceramic sheath does not show any deformation, cracking or bulging. The minimum wall thickness of the powder blade can be controlled within ±0.2mm, and there are no microcracks on the surface. However, the interior is not dense enough and the densification process is not completed. There are defects in the original powder particle boundaries and pores, which does not meet the internal metallurgical quality requirements of the blade.

[0115] Comparative Example 4 is a method for forming a powder high-temperature high-entropy alloy blade, which is different in that the SiC fiber mesh or C fiber mesh is not used for strengthening layer protection treatment. The specific steps are as follows:

[0116] (1) The nominal alloy composition is a powder high-temperature high-entropy alloy blade of Ni-Co-Fe-Cr-Al-Ti system, with a powder mean particle size D50 of 80 μm and a tap density of 5.2 g / cm 3 ; The minimum wall thickness of the blade is 1.2mm, the blade length is 95mm, and the torsion angle is 18°;

[0117] (2) Preparation of blade wax model: The wax model is prepared by 3D printing method, blue high-strength wax is used as the wax material, and the wax model is roughened;

[0118] (3) Preparation of ceramic jacket surface layer: Alumina and silica sol are mixed with a powder-liquid weight ratio of 1.3:1, and the slurry viscosity is controlled at 8s to obtain a surface coating. The surface coating is applied to the wax mold after roughening treatment, and then alumina sand is applied. After drying, the shell surface layer is obtained. Two layers of surface layer are prepared according to the above method, and the particle size of alumina is 200 mesh and the particle size of alumina sand is 160 mesh.

[0119] (4) Preparation of ceramic sheath back layer: bauxite powder and silica sol are mixed at a powder-liquid weight ratio of 1:1, stirred for 2 hours, and the slurry viscosity is controlled at 5-6 seconds to prepare the back layer slurry, which is applied to the shell surface layer, and then coated with back layer bauxite sand, and then slurried and dried. Four back layers are prepared according to the above method, with the particle size of bauxite powder being 160 mesh and the particle size of bauxite sand being 40 mesh;

[0120] (5) Firing after dewaxing of the ceramic sheath: dewaxing temperature 700°C, dewaxing time 2h, calcining temperature 1100°C, calcining time 3h;

[0121] (6) Ceramic sleeve cleaning: Use butanone to clean the wax mold to remove oil and impurities;

[0122] (7) Ceramic shell inspection: Use an endoscope to inspect the ceramic shell to see if there are cracks or bulges on the shell surface. The shell can only be used after the quality inspection is qualified.

[0123] (8) Powder packaging and degassing: high-temperature high-entropy alloy powders of different compositions are loaded into the mold shell described in step (7) for packaging and degassing;

[0124] (9) Hot isostatic pressing: Place the packaged shell into a hot isostatic pressing furnace at a hot isostatic pressing temperature of 1200°C, a pressure of 150 MPa, and a time of 2.5 h;

[0125] (10) Removal of ceramic sheath: First, mechanical water cleaning is used to remove the shell, and then chemical alkali boiling is used to remove the residual shell material. The alkali boiling liquid is sodium hydroxide;

[0126] (11) Powder blade inspection: The micro cracks on the blade surface are detected by fluorescence detection method, and then it is placed in ultrasonic testing equipment and combined with X-ray detection to evaluate its internal metallurgical quality. Finally, it is placed on a blue light scanner platform for dimensional contour scanning.

[0127] The results show that the powder high-temperature high-entropy alloy blade can be formed without microcracks on the surface, and without metallurgical defects such as pores and inclusions inside. The grains are fine, and the average grain size is 56μm, which can meet the metallurgical quality requirements of the internal and external blades. However, the strength of the ceramic sheath prepared by this method is only 3.0MPa. After hot isostatic pressing, the ceramic sheath is slightly deformed, resulting in an increase in the minimum wall thickness tolerance range of the powder blade from ±0.2mm to ±1mm; deformation occurs in the radial direction, and the torsion angle becomes larger. The measured value is 20°, which does not meet the design value.

[0128] The above embodiments are only used to help understand the method and core idea of ​​the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.

[0129] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for forming a powder high-temperature high-entropy alloy blade, comprising the following steps: S1) preparing a surface layer slurry on the surface of a blade wax mold, and then preparing aluminum oxide sand or silicon oxide sand on the surface, and drying to obtain a mold shell surface layer; The surface layer slurry includes one of aluminum oxide and silicon oxide, and a liquid binder; S2) preparing a backing slurry on the surface of the shell surface layer, and then preparing a backing refractory sand on the surface, and reinforcing it with a ceramic mesh, and obtaining a ceramic shell after drying; the backing slurry includes a refractory material and a liquid binder; S3) dewaxing and calcining the ceramic shell to obtain an initial shell; S4) placing the high temperature high entropy alloy powder in an initial mold shell for packaging, then performing hot isostatic pressing, and finally removing the surface mold shell to obtain a powder high temperature high entropy alloy blade.

2. The molding method according to claim 1, characterized in that: The high temperature high entropy alloy powder comprises Ni-Co-Fe-Cr-Al-Ti, the particle size of the high temperature high entropy alloy powder is 30-120 μm, and the tap density is 5.0-5.5 g / cm 3 .

3. The molding method according to claim 1, characterized in that: In step S1), the powder-liquid weight ratio of the surface layer slurry is 1.3:1 to 3:1, the viscosity is 5 to 30 seconds, and the liquid binder is silica sol; the particle size of one of the aluminum oxide and the silicon oxide is independently 200 to 325 mesh, the particle size of the aluminum oxide sand or the silicon oxide sand is 160 to 250 mesh, and the number of layers of the shell surface layer is 2 to 3 layers.

4. The molding method according to claim 1, characterized in that: In step S2), the refractory material is bauxite, the liquid binder is silica sol, the powder-liquid weight ratio of the back layer slurry is 1:1-1:3, the viscosity is 5-10s, and the number of back layers of the ceramic shell is 4-5.

5. The molding method according to claim 1, characterized in that: The ceramic mesh is a SiC fiber mesh or a C fiber mesh; the steps of reinforcing the ceramic mesh are specifically as follows: After preparing the second layer of back refractory sand, use ceramic mesh to reinforce it, dry it, and then prepare another back refractory sand, and then use ceramic mesh to reinforce it, dry it, and repeat this process several times until the last layer of ceramic mesh is reinforced and dried.

6. The molding method according to claim 1, characterized in that: The dewaxing temperature is 500-800° C., and the time is 1-2 hours; the calcining temperature is 1000-1500° C., and the time is 2-6 hours.

7. The molding method according to claim 1, characterized in that: In step S3), after the calcination, the process further comprises: The fired shell was cleaned with butanone and then subjected to endoscopic inspection.

8. The molding method according to claim 1, characterized in that: The hot isostatic pressing is performed at a temperature of 1100 to 1300° C., a pressure of 140 to 170 MPa, and a time of 2 to 5 hours.

9. The molding method according to claim 1, characterized in that: The method for removing the surface shell is specifically as follows: Mechanical water is first used for cleaning, and then chemical alkali boiling is used to remove the residual shell material, and the reagent for the alkali boiling is sodium hydroxide.

10. The molding method according to any one of claims 1 to 9, characterized in that: The wax model is prepared by a 3D printing method.