Preparation method of aluminum-based composite wire for realizing graphene directional arrangement through liquid-phase preparation process

Through liquid phase preparation technology and hot press sintering technology, combined with ammonia atmosphere and syringe spinning technology, the problem of directional arrangement of graphene in graphene/aluminum composite materials is solved, and high-performance graphene/aluminum composite materials are achieved Silk material preparation improves conductive and mechanical properties and reduces preparation costs.

CN118875284AActive Publication Date: 2024-11-01HARBIN INST OF TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410983894.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-01
Estimated Expiration
2044-07-22

AI Technical Summary

Technical Problem

The prior art cannot effectively control the orientation arrangement of graphene in graphene/aluminum composite materials, resulting in poor electrical conductivity and mechanical properties of the material and complex preparation process.

Method used

The liquid phase preparation process is adopted, through high-energy mechanical ball milling and hot press sintering technology, combined with densification treatment in ammonia atmosphere, AlN nanointerface layer is generated, and the directional arrangement of graphene is achieved with syringe spinning technology, and it is also in the molding coolant. Rapid cooling to improve material performance.

Benefits of technology

The high-quality and directional arrangement of graphene/aluminum composite wires is achieved, the conductive and mechanical properties are improved, the preparation cost is reduced, and the material has excellent tensile strength and corrosion resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118875284A_ABST
    Figure CN118875284A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a graphene aluminum-based composite wire, in particular to a preparation method of an aluminum-based composite wire with graphene directionally arranged through a liquid-phase preparation process. In order to solve the problem of disordered arrangement of graphene in a composite material and realize directional arrangement of graphene in a graphene / aluminum composite material wire, the invention provides an aluminum-based composite material wire preparation method for realizing directional arrangement of graphene through a liquid-phase preparation process. The graphene / aluminum precursor is subjected to densification hot pressed sintering in an ammonia gas-containing atmosphere to obtain a quasi-oriented arrangement graphene / aluminum preform cast ingot, and a C-N amorphous compound can inhibit interface reaction and fill holes and defects at an interface, so that the conductivity of the composite material is improved. And the adopted spinning nozzles are flat spinning nozzles, so that the graphene sheet layers can be regularly, uniformly and directionally arranged, and the orientation degree of the graphene sheet layers is improved. And the Na2CO3 forming cooling liquid is adopted, so that the corrosion resistance of the composite wire is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a graphene aluminum-based composite material wire. Background Art

[0002] Metal matrix composite wire is a composite fiber material composed of a metal matrix and other non-metallic materials. Metal matrix composite wire combines the high strength, heat resistance and conductivity of metal with the light weight and corrosion resistance of other materials, and has multiple excellent properties. The non-metallic material graphene has extremely high theoretical performance, with a tensile strength of more than 100GPa and an elastic modulus of up to 1TPa. It has received widespread attention since its birth. As an emerging high-performance reinforcement, graphene has very broad application prospects in the field of composite materials.

[0003] Graphene is often used in metal-based materials to enhance the performance of metal-based composite wires due to its unique two-dimensional strengthening characteristics. Directed graphene sheets can significantly enhance the electrical and thermal conductivity of composite materials and improve the strength of materials. However, the current mainstream hot pressing process and sintering process cannot control the arrangement of graphene when making graphene / aluminum composite materials, resulting in graphene being randomly dispersed in the matrix, which makes the arrangement of graphene sheets disorderly and disorderly. There are a large number of defects in the graphene / aluminum composite materials and leads to incomplete boundaries, thereby reducing the incompleteness and discontinuity of the electron transport path, thereby affecting the transport capacity of electrons in the composite material and reducing the electrical conductivity of the material. In addition, due to the disordered arrangement of graphene, the mechanical properties of graphene / aluminum composite materials are also poor, the strength, toughness and tensile properties of the materials are all affected, and the preparation process of the materials is complicated and the preparation difficulty is relatively large. Therefore, there is an urgent need for a preparation process that can make graphene in a graphene / aluminum composite wire be arranged in a directional manner. Summary of the invention

[0004] In order to solve the problem of disordered arrangement of graphene in composite materials and realize directional arrangement of graphene in graphene / aluminum composite wires, the present invention proposes a method for preparing aluminum-based composite wires with directional arrangement of graphene by a liquid phase preparation process.

[0005] The method for preparing aluminum-based composite wire with directional arrangement of graphene by liquid phase preparation process of the present invention is carried out in the following steps:

[0006] 1. Weighing

[0007] Weigh 0.5% to 2% of graphene and the remainder of aluminum metal powder as raw materials;

[0008] 2. Preparation of graphene / aluminum powder precursor

[0009] The graphene and aluminum metal powder weighed in step 1 are mixed and added to a ball mill for high-energy mechanical ball milling to obtain graphene-aluminum powder; the high-energy mechanical ball milling enables the graphene to be evenly dispersed on the surface of the aluminum powder and enables the graphene to have a strong mechanical bond with the aluminum metal powder, thereby obtaining a composite material powder with a strong physical bond of graphene-aluminum; the obtained graphene-aluminum powder is separated from the ball milling balls, and then the graphene-aluminum powder is loaded into a steel mold, and compacted by a hydraulic press to obtain a graphene / aluminum precursor with directional arrangement of graphene;

[0010] 3. Sintering of graphene / aluminum precursor under protective atmosphere

[0011] The graphene / aluminum precursor in step 2 is placed in an atmosphere furnace, the atmosphere furnace is sealed and evacuated, and then ammonia or a mixed atmosphere of ammonia and argon is filled into the atmosphere furnace, and hot pressing and sintering are performed to obtain a quasi-directionally arranged graphene / aluminum preform ingot; the ammonia or a mixed atmosphere of ammonia and argon can form AlN at the graphene-aluminum interface, and AlN has a hexagonal structure, which is convenient for interlayer slip. AlN connected at the graphene-aluminum matrix interface helps to coordinate the deformation of graphene and promote the directional arrangement of graphene;

[0012] The hot pressing sintering process is as follows: heating the furnace to 600-650°C at a heating rate of 5-10°C / min, then applying a pressure of 100-150MPa to the preform and hot pressing for 240-300 minutes, and finally obtaining a composite ingot of quasi-oriented graphene / aluminum after the temperature of the atmosphere furnace drops to room temperature;

[0013] The volume fraction of ammonia in the mixed atmosphere of ammonia and argon is 50%; ammonia and argon can better protect the material and prevent other mixed gases from polluting the composite material;

[0014] 4. Preparation of oriented graphene / aluminum composite wires

[0015] The liquid graphene / aluminum composite material obtained by heating the quasi-oriented graphene / aluminum preform ingot prepared in step 3 is added into a syringe, the nozzle of the syringe is placed in a molding coolant, the liquid graphene / aluminum composite material is extruded by the syringe and cooled in the molding coolant to obtain a composite material wire containing highly oriented graphene; the nozzle tube of the syringe is a flat nozzle tube or a round nozzle tube;

[0016] The solute in the molding coolant is Na2CO3;

[0017] 5. Annealing

[0018] The composite wire containing highly oriented graphene obtained in step 4 is subjected to annealing treatment. The annealing treatment is used to eliminate the residual stress in the wire after cooling, stabilize the grain size in the composite wire, reduce deformation and crack tendency, and improve material properties;

[0019] The present invention and its advantageous principles and beneficial effects:

[0020] 1. The present invention densifies and hot-presses a graphene / aluminum precursor in an atmosphere containing ammonia to obtain a quasi-oriented graphene / aluminum preform ingot. Ammonia decomposes active N atoms at high temperature to generate a nano-interface layer of AlN and CN amorphous compounds at the graphene-aluminum interface. AlN has a hexagonal structure and a strong basal plane slip characteristic, which can assist the coordinated deformation of graphene in the subsequent deformation process and better assist the oriented arrangement of graphene. The CN amorphous compound can inhibit the interface reaction, fill the holes and defects at the interface, thereby improving the conductive properties of the composite material, and realizing the preparation of high-quality, highly oriented graphene / aluminum composite wires.

[0021] 2. The present invention utilizes a liquid phase process to prepare oriented graphene / aluminum composite material filaments. The graphene / aluminum composite material ingot is melted into a molten liquid state, and then loaded into a syringe and extruded to form filaments. The equipment spinneret adopts a flat spinneret. The flat spinneret can induce two-dimensional graphene to be extruded parallel to the flat spinneret, so that the graphene sheets will be regularly and evenly oriented, thereby improving the orientation degree of the graphene sheets.

[0022] 3. The preparation of the composite material wire of the present invention does not require large plastic deformation treatment, and the manufacturing equipment used is simple, convenient and low-cost, so low-cost graphene / aluminum composite material wire manufacturing can be achieved.

[0023] 4. In the process of extruding the graphene / aluminum composite wire prepared by the present invention, the nozzle of the syringe is immersed in the cold coolant, and the graphene / aluminum composite material is rapidly cooled to achieve the quenching effect, thereby inhibiting the growth of aluminum grains during the slow cooling process, achieving the fine grain strengthening of the matrix in the composite material, and further enhancing the mechanical properties of the graphene / aluminum composite wire;

[0024] 5. In the present invention, a 5% Na2CO3 molding coolant is used to quickly cool the graphene / aluminum molten wire extruded from the nozzle of the syringe to achieve material shaping; the solvent of the molding coolant has a large specific heat capacity and does not react with molten aluminum, so that the aluminum wire can be cooled safely and efficiently; at the same time, the Na2CO3 solution is alkaline, and the alkaline substances therein can react chemically with the aluminum on the surface of the composite material, thereby forming a corrosion-resistant passivation film on the surface of the wire, thereby improving the corrosion resistance of the composite wire;

[0025] 6. The composite material wire prepared by the present invention has excellent performance, with a tensile strength of 550-700 MPa and an elongation of 13%-16%; the process is stable, the equipment is simple, and there is no pollution, so large-scale production can be achieved. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 is a schematic diagram of the structure of a syringe;

[0027] Figure 2 It is a schematic diagram of the structure of the flat nozzle tube of the syringe;

[0028] Figure 3 It is a schematic diagram of the structure of the circular nozzle tube of the syringe;

[0029] Figure 4 100 times metallographic image of the composite material wire prepared in Example 1;

[0030] Figure 5 XRD pattern of the composite material wire prepared in Example 1;

[0031] Figure 6 Macroscopic photograph of the composite material filament prepared in Example 1;

[0032] Figure 7 Macroscopic photograph of the composite material wire prepared in Example 2. DETAILED DESCRIPTION

[0033] The technical solution of the present invention is not limited to the specific implementation modes listed below, but also includes any reasonable combination of the specific implementation modes.

[0034] Specific implementation method 1: The method for preparing aluminum-based composite wire with directional arrangement of graphene by liquid phase preparation process in this implementation method is carried out in the following steps:

[0035] 1. Weighing

[0036] Weigh 0.5% to 2% of graphene and the remainder of aluminum metal powder as raw materials;

[0037] 2. Preparation of graphene / aluminum powder precursor

[0038] The graphene and aluminum metal powders weighed in step 1 are mixed and added to a ball mill for high-energy mechanical ball milling to obtain graphene-aluminum powder; the obtained graphene-aluminum powder is separated from the ball milling balls, and then the graphene-aluminum powder is loaded into a steel mold and compacted by a hydraulic press to obtain a graphene / aluminum precursor with directional graphene arrangement;

[0039] 3. Sintering of graphene / aluminum precursor under protective atmosphere

[0040] The graphene / aluminum precursor in step 2 is placed in an atmosphere furnace, the atmosphere furnace is sealed and evacuated, and then ammonia or a mixed atmosphere of ammonia and argon is filled into the atmosphere furnace for hot pressing and sintering to obtain a quasi-oriented graphene / aluminum preform ingot;

[0041] The hot pressing sintering process is as follows: heating the furnace to 600-650°C at a heating rate of 5-10°C / min, then applying a pressure of 100-150MPa to the preform and hot pressing for 240-300 minutes, and finally obtaining a composite ingot of quasi-oriented graphene / aluminum after the temperature of the atmosphere furnace drops to room temperature;

[0042] The volume fraction of ammonia in the mixed atmosphere of ammonia and argon is 50%;

[0043] 4. Preparation of oriented graphene / aluminum composite wires

[0044] The liquid graphene / aluminum composite material obtained by heating the quasi-oriented graphene / aluminum preform ingot prepared in step 3 is added into a syringe, the nozzle of the syringe is placed in a molding coolant, the liquid graphene / aluminum composite material is extruded by the syringe and cooled in the molding coolant to obtain a composite material wire containing highly oriented graphene; the nozzle tube of the syringe is a flat nozzle tube or a round nozzle tube;

[0045] The solute in the molding coolant is Na2CO3;

[0046] 5. Annealing

[0047] The composite material wire containing highly oriented graphene obtained in step 4 is annealed.

[0048] This implementation has the following beneficial effects:

[0049] 1. In this embodiment, the graphene / aluminum precursor is densified and hot-pressed in an atmosphere containing ammonia to obtain a quasi-oriented graphene / aluminum preform ingot. Ammonia decomposes active N atoms at high temperature to generate a nano-interface layer of AlN and CN amorphous compounds at the graphene-aluminum interface; AlN has a hexagonal structure and has a strong basal slip characteristic, which can assist the coordinated deformation of graphene in the subsequent deformation process and better assist the oriented arrangement of graphene; CN amorphous compounds can inhibit interfacial reactions, fill the holes and defects at the interface, thereby improving the conductive properties of the composite material, and realizing the preparation of high-quality, highly oriented graphene / aluminum composite wires.

[0050] 2. This embodiment uses a liquid phase process to prepare oriented graphene / aluminum composite material filaments. The graphene / aluminum composite ingot is melted into a molten liquid state, and then loaded into a syringe and extruded to form filaments. The equipment spinneret adopts a flat spinneret. The flat spinneret can induce two-dimensional graphene to be extruded parallel to the flat spinneret, so that the graphene sheets will be regularly and evenly oriented, thereby improving the orientation degree of the graphene sheets.

[0051] 3. The preparation of the composite material wire in this embodiment does not require large plastic deformation treatment, and the manufacturing equipment used is simple, convenient, and low-cost, so low-cost graphene / aluminum composite material wire manufacturing can be achieved.

[0052] 4. In the extrusion process of preparing the graphene / aluminum composite wire in this embodiment, since the nozzle of the syringe is immersed in the cold coolant, the graphene / aluminum composite material is quickly cooled to achieve the quenching effect, which inhibits the growth of aluminum grains during the slow cooling process, realizes the fine grain strengthening of the matrix in the composite material, and further enhances the mechanical properties of the graphene / aluminum composite wire;

[0053] 5. In this embodiment, a 5% Na2CO3 molding coolant is used to quickly cool the graphene / aluminum molten wire extruded from the nozzle of the syringe to achieve material shaping; the solvent of the molding coolant has a large specific heat capacity and does not react with molten aluminum, so that the aluminum wire can be safely and efficiently cooled; at the same time, the Na2CO3 solution is alkaline, and the alkaline substances therein can chemically react with the aluminum on the surface of the composite material, thereby forming a corrosion-resistant passivation film on the surface of the wire, thereby improving the corrosion resistance of the composite wire;

[0054] 6. The composite material wire prepared in this embodiment has excellent performance, with a tensile strength of 550-700 MPa and an elongation of 13%-16%. The process is stable, the equipment is simple, and there is no pollution, so large-scale production can be achieved.

[0055] Specific embodiment 2: This embodiment is different from specific embodiment 1 in that: the aluminum metal powder in step 1 is one or a combination of several of Al-Si alloy, Al-Si-Cu alloy, Al-Mg-Si alloy, Al-Cu-Mg alloy, Al-Zn-Cu alloy, Al-Zn-Mg-Cu alloy, Al-Si-Cu-Mg alloy;

[0056] The mass fraction of Si in Al-Si alloy is 2% to 25%;

[0057] The mass fraction of Si in Al-Mg-Si alloy is 0.5% to 25%, and the mass fraction of Mg is 0.5% to 50%;

[0058] The mass fraction of Si in Al-Si-Cu alloy is 0.5% to 25%, and the mass fraction of Cu is 0.5% to 53%;

[0059] The mass fraction of Cu in Al-Cu-Mg alloy is 0.5% to 53%, and the mass fraction of Mg is 0.5% to 38%;

[0060] The mass fraction of Zn in Al-Zn-Cu alloy is 0.5% to 55%, and the mass fraction of Cu is 0.5% to 53%;

[0061] The mass fraction of Zn in Al-Zn-Mg-Cu alloy is 0.5% to 55%, the mass fraction of Mg is 0.5% to 38%, and the mass fraction of Cu is 0.5% to 53%;

[0062] The mass fraction of Si in the Al-Si-Cu-Mg alloy is 0.5% to 25%, the mass fraction of Cu is 0.5% to 53%, and the mass fraction of Mg is 0.5% to 38%.

[0063] Specific implementation method three: This implementation method is different from specific implementation methods one or two in that: the compaction process in step two is: applying a longitudinal pressure of 60 to 80 KN and maintaining the pressure for 10 to 20 minutes.

[0064] Specific embodiment 4: This embodiment differs from specific embodiments 1 to 3 in that: the ball-to-material ratio in the high-energy mechanical ball milling process in step 2 is (8-15):1; the ball milling speed is from 200 to 300 r / min, and the ball milling time is 4 to 6 hours. A larger ball-to-material ratio can make the graphene distribution more uniform.

[0065] Specific implementation mode five: This implementation mode is different from any one of specific implementation modes one to four in that: the graphene described in step two is few-layer graphene with an average sheet diameter of 150 nm to 25 μm and an average thickness of 0.5 to 25 nm.

[0066] Specific embodiment 6: This embodiment is different from any one of specific embodiments 1 to 5 in that: the solvent in the molding coolant in step 4 is diesel or a mixed solvent obtained by mixing alkanes, cycloalkanes and aromatics in any proportion.

[0067] Specific embodiment seven: This embodiment differs from any one of specific embodiments one to six in that: the carbon number of alkanes, cycloalkanes or aromatics in the mixed solvent in step four is 9 to 18; the carbon number of alkanes, cycloalkanes or aromatics contained in the diesel is 9 to 18.

[0068] Specific implementation eight: This implementation differs from any one of specific implementations one to seven in that the mass fraction of Na2CO3 in the molding coolant in step four is 2-5%.

[0069] Specific embodiment 9: This embodiment is different from any one of specific embodiments 1 to 8 in that: the heating temperature of the quasi-oriented graphene / aluminum preform ingot in step 4 is 700-800°C.

[0070] Specific embodiment 10: This embodiment differs from any one of specific embodiments 1 to 9 in that: the syringe described in step 4 is composed of a syringe tube (1), a piston (2), a nozzle tube (3) and a spacer (4); the piston (2) is arranged in the syringe tube (1), and the nozzle tube (3) is arranged at the lower end of the syringe tube (1); the nozzle tube (3) is a flat nozzle tube or a circular nozzle tube, and a plurality of parallel spacers (4) are arranged in the circular nozzle tube to divide the circular nozzle tube into a plurality of flat small nozzles. The efficiency of filament formation can be improved, and the process requirements for the syringe equipment can be reduced;

[0071] Specific implementation eleven: The present implementation differs from specific implementations one to ten in that the annealing process described in step five is: keeping warm at 300° C. for 1 hour and cooling with the furnace.

[0072] Embodiment 1:

[0073] The method for preparing aluminum-based composite wires with directional arrangement of graphene by liquid phase preparation process in this embodiment is carried out in the following steps:

[0074] 1. Weighing

[0075] Weigh 1% of graphene and the rest of 6061 aluminum metal powder as raw materials;

[0076] 2. Preparation of graphene / aluminum powder precursor

[0077] The graphene and aluminum metal powders weighed in step 1 are mixed and added to a ball mill for high-energy mechanical ball milling to obtain graphene-aluminum powder; the obtained graphene-aluminum powder is separated from the ball milling balls, and then the graphene-aluminum powder is loaded into a steel mold and compacted by a hydraulic press to obtain a graphene / aluminum precursor with directional graphene arrangement;

[0078] The compaction process is: applying a longitudinal pressure of 70KN and maintaining the pressure for 20 minutes;

[0079] The ball-to-material ratio in the high-energy mechanical ball milling process is 10:1; the ball milling speed is 200 r / min, and the ball milling time is 6 hours; the ball milling process is forward-stop-reverse-stop, the forward or reverse time is 10 minutes, and the stop time is 20 minutes;

[0080] The graphene is a few-layer graphene with an average sheet diameter of 5 μm and an average thickness of 5 nm;

[0081] 3. Sintering of graphene / aluminum precursor under protective atmosphere

[0082] The graphene / aluminum precursor in step 2 is placed in an atmosphere furnace, the atmosphere furnace is sealed and evacuated, and then ammonia is filled into the atmosphere furnace for hot pressing and sintering to obtain a quasi-oriented graphene / aluminum preform ingot;

[0083] The hot pressing sintering process is as follows: heating the furnace to 650°C at a heating rate of 10°C / min, then applying a pressure of 100MPa to the preform and hot pressing for 300 minutes, and finally obtaining a composite ingot of quasi-oriented graphene / aluminum after the temperature of the atmosphere furnace drops to room temperature;

[0084] 4. Preparation of oriented graphene / aluminum composite wires

[0085] The liquid graphene / aluminum composite material obtained by heating the quasi-oriented graphene / aluminum preform ingot prepared in step 3 is added into a syringe, the nozzle of the syringe is placed in a molding coolant, the liquid graphene / aluminum composite material is extruded by the syringe and cooled in the molding coolant to obtain a composite material wire containing highly oriented graphene;

[0086] The solute in the molding coolant is Na2CO3, and the solvent is diesel; the mass fraction in the molding coolant is 3%;

[0087] The carbon number of the alkanes, cycloalkanes or aromatics contained in the diesel oil is 9 to 18;

[0088] The heating temperature of the quasi-oriented graphene / aluminum preform ingot is 750° C.

[0089] The nozzle tube of the syringe is a flat nozzle tube;

[0090] The syringe is composed of a syringe tube (1), a piston (2), a nozzle tube (3) and a spacer (4); the piston (2) is arranged in the syringe tube (1), and the nozzle tube (3) is arranged at the lower end of the syringe tube (1); the nozzle tube (3) is a flat nozzle tube;

[0091] 5. Annealing

[0092] The composite material wire containing highly oriented graphene obtained in step 4 is annealed; the annealing process is: keeping warm at 300° C. for 1 hour and cooling with the furnace.

[0093] Figure 4 100 times metallographic image of the composite material wire prepared in Example 1, Figure 1 It can be seen that the graphene in the material is oriented and densely organized; Figure 5XRD diagram of the composite material wire prepared in Example 1, Figure 5 It can be seen that an AlN interface layer is formed at the interface. The tensile strength of the graphene-aluminum composite fiber with directional graphene prepared in this embodiment reaches 577MPa, the elongation is 14.1%, and the fiber material exhibits good corrosion resistance; the composite fiber exhibits good performance as a whole.

[0094] Example 2

[0095] The method for preparing aluminum-based composite wires with directional arrangement of graphene by liquid phase preparation process in this embodiment is carried out in the following steps:

[0096] 1. Weighing

[0097] Weigh 2% of graphene and the rest of 6061 aluminum metal powder as raw materials;

[0098] 2. Preparation of graphene / aluminum powder precursor

[0099] The graphene and aluminum metal powders weighed in step 1 are mixed and added to a ball mill for high-energy mechanical ball milling to obtain graphene-aluminum powder; the obtained graphene-aluminum powder is separated from the ball milling balls, and then the graphene-aluminum powder is loaded into a steel mold and compacted by a hydraulic press to obtain a graphene / aluminum precursor with directional graphene arrangement;

[0100] The compaction process is: applying a longitudinal pressure of 75KN and maintaining the pressure for 15 minutes;

[0101] The ball-to-material ratio in the high-energy mechanical ball milling process is 15:1; the ball milling speed is 300 r / min, and the ball milling time is 4 hours; the ball milling process is forward-stop-reverse-stop, the forward or reverse time is 15 minutes, and the stop time is 15 minutes;

[0102] The graphene is a few-layer graphene with an average sheet diameter of 5 μm and an average thickness of 5 nm;

[0103] 3. Sintering of graphene / aluminum precursor under protective atmosphere

[0104] The graphene / aluminum precursor in step 2 is placed in an atmosphere furnace, the atmosphere furnace is sealed and evacuated, and then a mixed atmosphere of ammonia and argon is filled into the atmosphere furnace for hot pressing and sintering to obtain a quasi-oriented graphene / aluminum preform ingot;

[0105] The volume fraction of ammonia in the mixed atmosphere of ammonia and argon is 50%;

[0106] The hot pressing sintering process is as follows: heating the furnace to 600°C at a heating rate of 5°C / min, then applying a pressure of 150MPa to the preform and hot pressing for 300 minutes, and finally obtaining a composite ingot of quasi-oriented graphene / aluminum after the temperature of the atmosphere furnace drops to room temperature;

[0107] 4. Preparation of oriented graphene / aluminum composite wires

[0108] The liquid graphene / aluminum composite material obtained by heating the quasi-oriented graphene / aluminum preform ingot prepared in step 3 is added into a syringe, the nozzle of the syringe is placed in a molding coolant, the liquid graphene / aluminum composite material is extruded by the syringe and cooled in the molding coolant to obtain a composite material wire containing highly oriented graphene;

[0109] The solute in the molding coolant is Na2CO3, and the solvent is diesel; the mass fraction in the molding coolant is 3%;

[0110] The carbon number of the alkanes, cycloalkanes or aromatics contained in the diesel oil is 9 to 18;

[0111] The heating temperature of the quasi-oriented graphene / aluminum preform ingot is 700° C.

[0112] The nozzle tube of the syringe is a flat nozzle tube;

[0113] The syringe is composed of a syringe tube (1), a piston (2), a nozzle tube (3) and a spacer (4); the piston (2) is arranged in the syringe tube (1), and the nozzle tube (3) is arranged at the lower end of the syringe tube (1); the nozzle tube (3) is a flat nozzle tube;

[0114] 5. Annealing

[0115] The composite material wire containing highly oriented graphene obtained in step 4 is annealed; the annealing process is: keeping warm at 300° C. for 1 hour and cooling with the furnace.

[0116] The graphene-aluminum composite fiber with directional graphene prepared in this embodiment has a tensile strength of 618 MPa and an elongation of 13.6%; the composite fiber exhibits good tensile properties and elongation.

Claims

1. A method for preparing aluminum-based composite wire with directional arrangement of graphene by liquid phase preparation process, characterized in that: The preparation method of aluminum-based composite wire with directional arrangement of graphene by liquid phase preparation process is carried out in the following steps:

1. Weighing Weigh 0.5% to 2% of graphene and the remainder of aluminum metal powder as raw materials; 2. Preparation of graphene / aluminum powder precursor The graphene and aluminum metal powders weighed in step 1 are mixed and added to a ball mill for high-energy mechanical ball milling to obtain graphene-aluminum powder; the obtained graphene-aluminum powder is separated from the ball milling balls, and then the graphene-aluminum powder is loaded into a steel mold and compacted by a hydraulic press to obtain a graphene / aluminum precursor with directional graphene arrangement; 3. Sintering of graphene / aluminum precursor under protective atmosphere The graphene / aluminum precursor in step 2 is placed in an atmosphere furnace, the atmosphere furnace is sealed and evacuated, and then ammonia or a mixed atmosphere of ammonia and argon is filled into the atmosphere furnace for hot pressing and sintering to obtain a quasi-oriented graphene / aluminum preform ingot; The hot pressing sintering process is as follows: heating the furnace to 600-650°C at a heating rate of 5-10°C / min, then applying a pressure of 100-150MPa to the preform and hot pressing for 240-300 minutes, and finally obtaining a composite ingot of quasi-oriented graphene / aluminum after the temperature of the atmosphere furnace drops to room temperature; The volume fraction of ammonia in the mixed atmosphere of ammonia and argon is 50%; 4. Preparation of oriented graphene / aluminum composite wires The liquid graphene / aluminum composite material obtained by heating the quasi-oriented graphene / aluminum preform ingot prepared in step 3 is added into a syringe, the nozzle of the syringe is placed in a molding coolant, the liquid graphene / aluminum composite material is extruded by the syringe and cooled in the molding coolant to obtain a composite material wire containing highly oriented graphene; the nozzle tube of the syringe is a flat nozzle tube or a round nozzle tube; The solute in the molding coolant is Na2CO3; 5. Annealing The composite material wire containing highly oriented graphene obtained in step 4 is annealed.

2. The method for preparing aluminum-based composite wire with oriented graphene arranged by the liquid phase preparation process according to claim 1, characterized in that: The aluminum metal powder in step 1 is one or a combination of Al-Si alloy, Al-Si-Cu alloy, Al-Mg-Si alloy, Al-Cu-Mg alloy, Al-Zn-Cu alloy, Al-Zn-Mg-Cu alloy, Al-Si-Cu-Mg alloy; The mass fraction of Si in Al-Si alloy is 2% to 25%; The mass fraction of Si in Al-Mg-Si alloy is 0.5% to 25%, and the mass fraction of Mg is 0.5% to 50%; The mass fraction of Si in Al-Si-Cu alloy is 0.5% to 25%, and the mass fraction of Cu is 0.5% to 53%; The mass fraction of Cu in Al-Cu-Mg alloy is 0.5% to 53%, and the mass fraction of Mg is 0.5% to 38%; The mass fraction of Zn in Al-Zn-Cu alloy is 0.5% to 55%, and the mass fraction of Cu is 0.5% to 53%; The mass fraction of Zn in Al-Zn-Mg-Cu alloy is 0.5% to 55%, the mass fraction of Mg is 0.5% to 38%, and the mass fraction of Cu is 0.5% to 53%; The mass fraction of Si in the Al-Si-Cu-Mg alloy is 0.5% to 25%, the mass fraction of Cu is 0.5% to 53%, and the mass fraction of Mg is 0.5% to 38%.

3. The method for preparing aluminum-based composite wire with oriented graphene arranged by liquid phase preparation process according to claim 1, characterized in that: The compaction process in step 2 is: applying a longitudinal pressure of 60 to 80 KN and maintaining the pressure for 10 to 20 minutes.

4. The method for preparing aluminum-based composite wire with oriented graphene arranged by liquid phase preparation process according to claim 1, characterized in that: In step 2, the ball-to-material ratio in the high-energy mechanical ball milling process is (8-15):1; the ball milling speed is from 200 to 300 r / min, and the ball milling time is 4 to 6 hours.

5. The method for preparing aluminum-based composite wire with oriented graphene arranged by liquid phase preparation process according to claim 1, characterized in that: The graphene in step 2 is a few-layer graphene with an average sheet diameter of 150nm to 25μm and an average thickness of 0.5 to 25nm.

6. The method for preparing aluminum-based composite wire with oriented graphene arranged by liquid phase preparation process according to claim 1, characterized in that: The solvent in the molding coolant in step 4 is diesel or a mixed solvent obtained by mixing alkanes, cycloalkanes and aromatics in any proportion.

7. The method for preparing aluminum-based composite wire with oriented graphene arranged by liquid phase preparation process according to claim 1, characterized in that: In step 4, the carbon number of alkanes, cycloalkanes or aromatics in the mixed solvent is 9 to 18; the carbon number of alkanes, cycloalkanes or aromatics in the diesel is 9 to 18.

8. The method for preparing aluminum-based composite wire with oriented graphene arranged by liquid phase preparation process according to claim 1, characterized in that: The mass fraction of Na2CO3 in the molding coolant in step 4 is 2-5%.

9. The method for preparing aluminum-based composite wire with oriented graphene arranged by liquid phase preparation process according to claim 1, characterized in that: The heating temperature of the quasi-oriented graphene / aluminum preform ingot in step 4 is 700-800°C.

10. The method for preparing aluminum-based composite wire with oriented graphene arrangement by liquid phase preparation process according to claim 1, characterized in that: Step 4: The syringe is composed of a syringe tube (1), a piston (2), a nozzle tube (3) and a septum (4); The piston (2) is arranged in the injector tube (1), and the nozzle tube (3) is arranged at the lower end of the syringe tube (1); the nozzle tube (3) is a flat nozzle tube or a circular nozzle tube, and a plurality of parallel spacers (4) are arranged in the circular nozzle tube to divide the circular nozzle tube into a plurality of flat small nozzles.

Citation Information

Patent Citations

  • Graphene / copper composite and preparation method thereof

    CN104711443A

  • Graphene / nickel composite material and preparation method thereof

    CN105838913A

  • Graphene / aluminum-matrix composite for high-speed impact resistance and preparation method thereof

    CN109722556A

  • Atmosphere control powder metallurgy preparation method of graphene reinforced aluminum matrix composite

    CN113355548A

  • Chemical-free production of graphene-reinforced inorganic matrix composites

    US20170225233A1