NiCoCrAlY bonding layer microstructure femtosecond laser processing method

Through finite element software and dual-temperature equation simulation, the thermally affected zone and defect problems of NiCoCrAlY metal bonding layer are solved by femtosecond laser processing, and fine processing without thermal damage is achieved, and the mechanical bonding of the coating is enhanced. and service performance.

CN118875498APending Publication Date: 2024-11-01SICHUAN UNIV
View PDF 0 Cites 12 Cited by

Patent Information

Application Number
CN202410960294.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Prior Art When femtosecond laser processing of NiCoCrAlY metal bonding layer in the thermal barrier coating of turbine blades, processing defects such as heat-affected zones, microcracks and molten droplets are prone to occur, resulting in coating failure and falling off, and lack of high quality. Precision processing method.

Method used

The ablation model of NiCoCrAlY material is established through finite element software, combined with the dual-temperature equation for simulation, optimize the laser process parameters, and achieve fine processing without thermal damage. The specific steps include establishing an ablation model, setting the heat source add-on and Boundary conditions, ablation simulation, determine the laser energy density, scanning speed and number of scans to avoid processing defects.

Benefits of technology

High-quality microstructure processing without obvious heat-affected zones, no microcracks, no holes, and no molten droplets is achieved, which improves the mechanical bonding between the coating and the metal matrix and ensures the service performance of the coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118875498A_ABST
    Figure CN118875498A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of femtosecond laser processing, and particularly discloses a femtosecond laser processing method for a NiCoCrAlY bonding layer microstructure, which comprises the following steps: establishing an ablation model for femtosecond laser processing of a NiCoCrAlY material; ablating a heat source loading item of the model; setting boundary conditions; simulating an ablated NiCoCrAlY metal bonding layer in combination with a double-temperature equation; and laser process parameters are determined according to a simulation result, and thermal-damage-free femtosecond laser processing is carried out. According to the method, the dynamic conditions of temperature distribution and energy exchange of the NiCoCrAlY metal bonding layer processed by femtosecond laser are obtained by utilizing finite element software, the ablation influence of different laser process parameters on a material is predicted, the three-dimensional shape generated by ablation is obtained, the method is combined with experiments, the laser process parameters are determined through optimization, and finally, the effect of non-obvious heat affected zone, non-obvious heat affected zone and non-obvious heat affected zone are achieved. And precision machining is achieved without machining defects such as micro cracks, holes and molten drops. The problems of machining defects such as heat affected zones, remelting layers and microcracks possibly occurring in femtosecond laser machining in the prior art are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of femtosecond laser processing, and in particular to a femtosecond laser processing method for a NiCoCrAlY bonding layer microstructure. Background Art

[0002] With the development of aircraft engines, aircraft engines have put forward higher requirements for service life, efficiency, fuel consumption and thrust-to-weight ratio. At present, the maximum operating temperature of nickel-based high-temperature alloys used in hot end components is about 1080℃, while the inlet temperature of aircraft engines currently in service has reached 1727℃. In this case, a technology that can reduce the surface temperature of blades-thermal barrier coating technology has attracted the attention of researchers at home and abroad. Thermal barrier coatings are generally a multi-layer structural system composed of a ceramic layer, a thermally grown oxide layer, a bonding layer and a high-temperature alloy substrate. In the traditional process of preparing thermal barrier coatings, degreasing and sandblasting processes are often used before thermal spraying. The degreasing agent induces chemical modification of the surface and removes organic matter on the surface, while sandblasting changes the surface morphology by generating random roughness, thereby promoting the mechanical anchoring of the incoming particles on the substrate. Although such a process is very effective for most materials, there may be a risk of microcrack nucleation on the surface, and the appearance of inclusions will reduce the adhesion of subsequent coatings. In addition, during the service process, large thermal stress is easily generated at the interface, resulting in coating failure, and then the coating fails and falls off. In order to avoid failure and peeling of blade thermal barrier coating due to insufficient adhesion and to ensure the service performance of blade thermal barrier coating, the method of laser surface texturing is considered to improve the mechanical bonding strength between the coating and the metal substrate.

[0003] However, LST technology has high requirements for high-precision texture grooves, which directly affects the performance and function of the material surface. Precise control of laser parameters in LST processing is the key to achieving high-performance textures. For the thermal barrier coating system of turbine blades, it is necessary to conduct ablation experiments on the materials of different layers to ensure that the designed geometric dimensions and surface quality are achieved with high efficiency, and the processed surface is smooth without unnecessary heat-affected zones or damage, avoiding defects such as melt accumulation or microcracks. However, current research has little research on femtosecond laser processing of NiCoCrAlY materials, the metal bonding layer in the thermal barrier coating system of turbine blades. Therefore, there is an urgent need for a method that can achieve fine processing of NiCoCrAlY metal bonding layer coatings without thermal damage. Summary of the invention

[0004] In order to solve the problems existing in the prior art, the present invention provides a femtosecond laser processing method for a NiCoCrAlY bonding layer microstructure, and uses finite element software to obtain the temperature distribution and energy exchange dynamics of the NiCoCrAlY metal bonding layer processed by femtosecond laser, predict the influence of different laser process parameters on the ablation of the material, and obtain the three-dimensional morphology produced by the ablation. Combined with the experiment, by optimizing the laser process parameters, precise processing without obvious heat-affected zone, microcracks, holes, molten droplets and other processing defects is finally achieved; the process parameters obtained by the method of the present invention can be directly used to guide the femtosecond laser processing of the NiCoCrAlY metal bonding layer in the turbine blade, and solve the processing defects such as heat-affected zone, remelted layer, microcracks and the like that may occur in femtosecond laser processing.

[0005] To achieve the above object, the present invention provides the following technical solution: a femtosecond laser processing method for a NiCoCrAlY bonding layer microstructure, comprising the following steps:

[0006] S1. Establish the ablation model of NiCoCrAlY material processed by femtosecond laser;

[0007] S2, heat source add-on for ablation model;

[0008] S3, setting of boundary conditions;

[0009] S4, simulation of ablated NiCoCrAlY metal bonding layer combined with dual-temperature equation;

[0010] S5. Determine laser process parameters through simulation results and perform femtosecond laser processing without thermal damage.

[0011] Preferably, in step S1, numerical simulation software is used to model the bonding layer of the turbine NiCoCrAlY metal material, and the ablation model is a three-dimensional geometric model with a size of 300μm×300μm×100μm in the xyz direction; an adaptive strategy is adopted for mesh division, and free tetrahedral mesh is used for division to adapt to complex geometric shapes and boundary conditions; a distributed mesh density is used in the z direction, specifically including: a fine mesh is used in the area close to the surface, i.e., 0-20μm, and the mesh density is gradually reduced in the depth direction, i.e., 20-100μm; a uniform mesh is used in the surface area, i.e., 0-300μm, in the x and y directions.

[0012] Preferably, in step S2, the heat source loading term adopts a transient physical field method, and the upper surface of the geometric model is used as the loading surface of the laser heat source. The laser beam is vertically incident on the surface and distributes its energy in the ablation area. On the plane, the heat source term adopts a two-dimensional Gaussian distribution, and in the depth direction, the heat source term adopts an exponential decay form; the laser energy distribution function S acting on the surface of the metal material is specifically expressed as follows:

[0013]

[0014] Where R represents the temperature-dependent interface reflectivity of the surface, F0 is the laser peak energy density, and τ p is the laser pulse width, t0 is the position of the first laser peak in the time domain, w0 is the pulse laser focus spot radius, and α(x, y, z, t) is the laser absorption coefficient.

[0015] Preferably, in step S3, in order to accurately simulate the boundary conditions of heat conduction during femtosecond laser ablation, each boundary surface of the model is set respectively, and the surrounding boundaries and the bottom surface of the model are set to a constant temperature of 300K, and the heat flux is zero, that is, no heat is dissipated outward through these surfaces; the boundary condition formula is expressed as follows:

[0016]

[0017]

[0018] Among them, T e , T l They represent the transient temperatures of the electronic system and the lattice system respectively, k is the thermal conductivity, Q0 represents the heat source on the surface of the electronic system, and l represents the side length of the simulation model.

[0019] Preferably, in step S4, the following is specifically included:

[0020] S41. The dual-temperature equation is used to simulate the established femtosecond laser processing NiCoCrAlY material ablation model;

[0021] S42. Using different femtosecond laser process parameters, i.e., different laser energy densities, laser scanning speeds, and different repeated scanning times, to simulate the ablation of the NiCoCrAlY metal bonding layer, the temporal and spatial distribution of the electron temperature inside the material, the temporal and spatial distribution of the lattice temperature inside the material, the energy exchange process between the electronic system and the lattice system and its influencing factors, and the overall thermal response behavior of the material under the action of the femtosecond laser pulse, including the heating, cooling, and thermal diffusion processes;

[0022] S43. Through simulation analysis, the temperature distribution and energy exchange dynamics of the NiCoCrAlY metal bonding layer processed by femtosecond laser are obtained, the influence of different laser process parameters on the ablation of the material is predicted, and the three-dimensional morphology produced by the ablation is obtained.

[0023] Preferably, in step S41, the energy transfer between the electron and lattice system is described by a two-temperature equation to accurately reflect the thermal effect of the interaction between the femtosecond laser and the material; in the two-temperature equation, the electron system and the lattice system have different temperature fields, respectively, and the evolution of the two temperature fields is controlled by the following two coupled partial differential equations, and the control equations are expressed as follows:

[0024]

[0025] Among them, the subscripts e and l represent electrons and lattices respectively, C represents heat capacity, G is the electron-lattice coupling coefficient, and S represents the laser energy distribution function acting on the surface of the metal material.

[0026] Preferably, in step S5, based on the simulation analysis results of laser processing of NiCoCrAlY material, the laser process parameters are optimized and determined by achieving the processing purpose of having no obvious heat-affected zone, no microcracks, no holes, and no molten droplets in the coating; and the determined laser process parameters are used to achieve femtosecond laser fine processing of the NiCoCrAlY metal bonding layer coating without thermal damage.

[0027] Preferably, the determined laser process parameters specifically refer to: 2.831-3.137 J / cm 2 The laser energy density is 800-1000mm / s, the laser scanning speed is 800-1000mm / s, and the laser cycle scanning times are 40-45 times.

[0028] Preferably, the determined laser process parameters specifically refer to: 2.831 J / cm 2 The laser energy density is 800mm / s, the laser scanning speed is 800mm / s and the number of laser cycle scanning is 40 times.

[0029] The beneficial effects of the present invention are as follows: the present invention has good processing effect and precision. Through the simulation calculation of femtosecond laser ablation of NiCoCrAlY metal bonding layer, the non-equilibrium thermodynamic behavior of femtosecond laser acting on the material is described. The ablation simulation based on the dual-temperature model captures the dynamic evolution of the electronic and lattice non-equilibrium state of the material, and obtains the basic physical process of the interaction between the laser and the material, including the ablation morphology, heat accumulation and temperature distribution. Through simulation combined with experiments, the ablation mechanism of NiCoCrAlY material processed by laser is obtained. At 2.831J / cm 2 With a laser energy density of 800 mm / s, a laser scanning speed of 800 mm / s and 40 laser cycle scanning times, high-quality microstructure grooves with smooth processing walls, no obvious heat-affected zone, no microcracks, holes, molten droplets and other processing defects are obtained, realizing fine processing of the coating without thermal damage. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 A schematic diagram of the finite element mesh and boundary conditions of the simulation area in an embodiment of the present invention;

[0031] Figure 2 This is a diagram of heat accumulation of femtosecond laser multi-pulses in an embodiment of the present invention;

[0032] Figure 3 The simulated cross-sectional diagram of the femtosecond laser ablation of the NiCoCrAlY metal bonding layer at different laser energy densities in the embodiment of the present invention, (a) is 1.948 J / cm 2 , (b) is 2.831 J / cm 2 , (c) is 3.737 J / cm 2 , (d) is 4.521 J / cm 2 ;

[0033] Figure 4 The simulated cross-sectional views of the femtosecond laser ablation of the NiCoCrAlY metal bonding layer at different laser scanning speeds in the embodiment of the present invention are as follows: (a) is 600 mm / s, (b) is 800 mm / s, (c) is 1000 mm / s, and (d) is 1200 mm / s;

[0034] Figure 5 The simulated cross-sectional views of the femtosecond laser ablation of the NiCoCrAlY metal bonding layer at different laser scanning times in the embodiment of the present invention, (a) is 30 times, (b) is 40 times, (c) is 50 times, and (d) is 60 times;

[0035] Figure 6 A schematic diagram of a femtosecond laser processing device in an embodiment of the present invention;

[0036] Figure 7 Figure 2 is a top view of the femtosecond laser ablation experiment of NiCoCrAlY metal bonding layer at different laser energy densities in the embodiment of the present invention, (a) is 1.948 J / cm 2 , (b) is 2.831 J / cm 2 , (c) is 3.737 J / cm 2 , (d) is 4.521 J / cm 2 ;

[0037] Figure 8 The top view of the femtosecond laser ablation experiment of NiCoCrAlY metal bonding layer at different laser scanning speeds in the embodiment of the present invention, (a) is 600 mm / s, (b) is 800 mm / s, (c) is 1000 mm / s, and (d) is 1200 mm / s;

[0038] Fig. 9The top view of the femtosecond laser ablation experiment of NiCoCrAlY metal bonding layer with different laser scanning times in the embodiment of the present invention, (a) is 30 times, (b) is 40 times, (c) is 50 times, and (d) is 60 times;

[0039] Fig.10 Schematic diagram of the surface microstructure of the NiCoCrAlY metal bonding layer in an embodiment of the present invention, (a) is a top view SEM diagram of the microstructure, and (b) is a cross-sectional SEM diagram of the microstructure;

[0040] Fig.11 Schematic diagram of the three-dimensional contour morphology of the surface microstructure of the NiCoCrAlY metal bonding layer in an embodiment of the present invention, (a) is a schematic diagram of the three-dimensional contour morphology, and (b) is a schematic diagram of the two-dimensional cross-sectional morphology. DETAILED DESCRIPTION

[0041] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0042] As a high-temperature alloy, NiCoCrAlY has excellent high-temperature stability and oxidation resistance, but its material properties make it prone to defects such as heat-affected zones and microcracks during femtosecond laser processing. This requires detailed research and modeling of the material's thermophysical properties. Femtosecond laser processing requires extremely high precision and control, especially in the setting of parameters such as the number of scans, power density, and scanning speed. The slightest carelessness may lead to processing defects. At the same time, in order to avoid cracks, coating shedding, and remelting layers caused by inappropriate laser parameters when processing turbine blade air film holes by femtosecond laser, it is necessary to optimize the laser process parameters for different layers. Therefore, for the thermal barrier coating system of turbine blades, it is necessary to conduct ablation experiments on the materials of different layers to ensure that the designed geometric dimensions and surface quality are achieved with high efficiency, the processed surface is smooth and has no unnecessary heat-affected zones or damage, and defects such as melt accumulation or microcracks are avoided. However, there are few existing studies on NiCoCrAlY turbine blade metal bonding coatings. Therefore, laser parameter optimization for NiCoCrAlY material has high technical difficulty. Establishing an accurate ablation model and setting appropriate heat source add-ons and boundary conditions are crucial to the accuracy of the results.

[0043] The present invention adopts a dual-temperature equation (also called a dual-temperature model) to describe the energy exchange process between electrons and lattices when femtosecond laser ablate metal materials, and obtains the temperature distribution, dynamic situation of energy exchange and three-dimensional morphology produced by ablation during laser processing. According to the femtosecond laser processing technology theory and practical experience, numerical simulation software is used to model the turbine NiCoCrAlY metal bonding layer, mesh division, establishment of boundary conditions, laser body heat source loading and establishment of boundary conditions, and simulation calculation of femtosecond laser ablation of NiCoCrAlY materials is performed to provide theoretical guidance for ablation experiments. The NiCoCrAlY metal bonding layer is ablated by simulating different femtosecond laser process parameters (including laser energy density, laser scanning speed, and number of repeated scans). Since the laser ablation of NiCoCrAlY coating adopts a reciprocating scanning method of scribing, the heat energy of the laser accumulates in the material. This heat accumulation will cause local overheating of the material, thereby melting and resolidification in the ablation area. The simulation results of femtosecond laser multi-pulse ablation are compared and analyzed to select the optimal laser processing parameters to avoid the phenomenon of coating surface melting or oxidation during multi-pulse ablation.

[0044] See also Figure 1-Figure 11 The present invention provides a technical solution: a femtosecond laser processing method for the microstructure of a NiCoCrAlY bonding layer, using numerical simulation software Multiphysics established an ablation model for femtosecond laser processing of NiCoCrAlY materials and studied the dynamics of temperature distribution and energy exchange during laser processing. It can evaluate the influence of different laser process parameters on the ablation process, predict the material removal rate and the three-dimensional morphology produced by ablation, and adjust the process parameters of femtosecond laser processing based on this to achieve fine processing of NiCoCrAlY metal bonding layer coating without thermal damage, including the following steps:

[0045] Establishment of ablation model for femtosecond laser processing of NiCoCrAlY material

[0046] Numerical simulation software was used to model the bonding layer of the turbine NiCoCrAlY metal material. The ablation model is a three-dimensional geometric model with a geometric size of 300μm (x direction) × 300μm (y direction) × 100μm (z direction) to ensure that the microstructural features produced during the laser ablation process can be captured. NiCoCrAlY alloy was selected as the material of the model, and its thermophysical parameters and optical parameters were input to accurately simulate the interaction between the laser and the material. In order to improve the calculation accuracy and efficiency, an adaptive strategy was adopted for meshing, using free tetrahedral meshes for meshing to adapt to complex geometric shapes and boundary conditions. Figure 1As shown in the figure, a distributed grid density is used in the z direction (i.e., thickness direction). Specifically, a fine grid is used in the area close to the surface (0-20μm) to capture the subtle thermal effects and phase change processes generated during femtosecond laser ablation. The grid density is gradually reduced in the depth direction (20-100μm) to reduce the amount of calculation. Uniform grid division is used in the surface area (0-300μm×0-300μm) in the x and y directions to ensure that the energy distribution of the laser and its impact on the material can be accurately simulated in the ablation area.

[0047] Heat Source Add-In for Ablation Models

[0048] In the simulation of femtosecond laser ablation, it is crucial to accurately describe the heat source loading. In order to reflect the actual interaction between the laser and the material, the heat source loading term is described in a transient physical field manner. The upper surface of the geometric model (z = 0 plane) is used as the loading surface of the laser heat source. The laser beam is incident vertically on the surface and distributes its energy in the ablation area. In the plane (x, y direction), the heat source adopts a two-dimensional Gaussian distribution. In the depth direction (z direction), considering the absorption and attenuation of the laser, the heat source term adopts an exponential decay form. Specifically, S is the laser energy distribution function acting on the surface of the metal material, and the specific expression is shown in equation (1).

[0049]

[0050] Where R represents the temperature-dependent interface reflectivity of the surface, F0 is the laser peak energy density, τ p is the laser pulse width, t0 is the position of the first laser peak in the time domain, w0 is the pulse laser focus spot radius, and α(x, y, z, t) is the laser absorption coefficient, which is an optical property related to material temperature.

[0051] Setting boundary conditions

[0052] In order to accurately simulate the boundary conditions of heat conduction during femtosecond laser ablation, the boundary surfaces of the model were reasonably set. The boundaries (x=0, x=max, y=0, y=max) and the bottom surface (z=0) of the model were set to a constant temperature of 300K, and the heat flux was zero, that is, no heat was dissipated outward through these surfaces. The upper surface (z=0) of the geometric model is the laser body heat source loading surface. The input ablation source on the surface of the electronic system is set to a laser heat source, and the energy transfer on the surface of the lattice system is carried out through the collision between electrons and the lattice. The boundary conditions are set as equations (2) to (5).

[0053]

[0054] Among them, T e , T lThey represent the transient temperature of the electronic system and the lattice system, respectively, k is the thermal conductivity, Q0 represents the heat source on the surface of the electronic system, and l represents the side length of the simulation model. The visualization model established by Multiphysics can simplify the interaction process between laser and metal materials, and can efficiently explore the effects of different parameters such as laser power, pulse duration and material properties on the ablation process.

[0055] Simulation of Ablated NiCoCrAlY Metal Bonding Layer Combined with Dual-Temperature Equation

[0056] The dual-temperature equation is used to simulate the established femtosecond laser processing NiCoCrAlY material ablation model:

[0057] The two-temperature model (TTM) is used to simulate the processing morphology, thermal damage mechanism and optimization of laser processing technology of NiCoCrAlY coating during femtosecond laser processing. The model can accurately reflect the thermal effect of the interaction between femtosecond laser and material by describing the energy transfer between the electron and lattice systems. In the two-temperature model, the electron system and the lattice system have different temperature fields respectively. The evolution of these two temperature fields is controlled by the following two coupled partial differential equations. The control equations are expressed as equations (6) and (7):

[0058]

[0059] Among them, the subscripts e and l represent electrons and lattices respectively, C represents heat capacity, G is the electron-lattice coupling coefficient, k is thermal conductivity, and T e and T l They represent the transient temperatures of the electronic system and the lattice system respectively, and S represents the laser energy distribution function acting on the surface of the metal material.

[0060] After modeling and analysis based on the dual-temperature model, the thermal response behavior of the NiCoCrAlY material is obtained, describing the ultrafast electron-lattice energy exchange, heat conduction and other phenomena, and simulating the temperature change process of the electron and lattice system in the NiCoCrAlY material under the action of femtosecond laser pulses. The process parameters include laser energy density, laser scanning speed, and repeated scanning times. The ablation simulation of the NiCoCrAlY metal bonding layer is carried out using different femtosecond laser process parameters, namely different laser energy density, laser scanning speed, and different repeated scanning times; the time and space distribution of the electron temperature inside the material, the time and space distribution of the lattice temperature inside the material, the energy exchange process between the electronic system and the lattice system and its influencing factors, and the overall thermal response behavior of the material under the action of femtosecond laser pulses, including heating, cooling and thermal diffusion processes, are obtained. Figure 2As shown, it can be observed that the energy deposition of multiple pulses on the coating surface causes the temperature to rise. The pulse time interval of the incident laser limits the heat diffusion process, and the coating surface temperature drops rapidly, and cools down before the arrival of the next pulse.

[0061] The results of different laser energy density, laser scanning speed and different scanning times are as follows Figure 3 , Figure 4 and Figure 5 As shown in the figure, the temperature cloud map can be used to find the range of the heat-affected zone and the change in surface temperature gradient, and it can be predicted that the simulated theoretical model and calculation method can effectively simulate the actual femtosecond laser ablation process. Through the simulation results, the femtosecond laser processing parameters can be optimized, the processing quality and efficiency can be improved, especially the precise control of the ablation morphology, which provides a theoretical basis for the application of femtosecond laser in material surface modification and performance improvement. Figure 3 (a) Figure 3 (b) Figure 3 (c) Figure 3 (d) represents 1.948 J / cm 2 , 2.831J / cm 2 , 3.737J / cm 2 and 4.521 J / cm 2 The ablation simulation of NiCoCrAlY metal bonding layer under laser energy density of 4.521 J / cm2 shows that the width and depth of the groove increase with the increase of laser energy density. The temperature cloud map shows that the heat affected zone usually shows the characteristics of the high temperature area gradually transitioning to the surrounding lower temperature area. In addition, with the increase of laser energy density, the temperature gradient of the groove surface changes significantly. When the laser energy density is 4.521 J / cm2, the groove surface temperature gradient ... 2 When the laser is used, the area with the greatest temperature impact is located on the surface of the groove sidewall. Although the heat affected zone of the femtosecond laser is relatively small, as the energy density increases, the heat propagation to the surrounding materials becomes more significant. The material will not only be ablated, but also melted. This molten material will quickly cool and resolidify after the laser pulse to form a molten layer. This process is particularly obvious on the walls and bottom of the groove because these areas accumulate more heat under the action of continuous lasers. The simulation results verify the formation mechanism of the heat affected zone during the ablation experiment. Although the pulse of the femtosecond laser is very short and can locally concentrate energy to generate high temperature, some heat still diffuses to the surrounding materials through heat conduction, causing the temperature of the groove wall to rise. In addition, the action of repeated pulses may cause the temperature of these areas to further increase, thus forming a heat affected zone.

[0062] Figure 4 (a) Figure 4 (b) Figure 4 (c) Figure 4(d) represents the ablation simulation of NiCoCrAlY metal bonding layer under laser scanning speeds of 600mm / s, 800mm / s, 1000mm / s and 1200mm / s, respectively. When the scanning speed is reduced, the temperature of the groove wall is higher. Due to the prolonged interaction time between the laser and the material, the accumulation of heat energy in the material is more significant. According to Fourier's law of heat conduction, the heat energy propagates inside the material along the temperature gradient, resulting in an increase in the temperature of the groove wall. This heat accumulation causes the heat to exceed the thermal diffusion capacity of the material, forming a local heat-affected zone. With the increase of the scanning speed, the surface cumulative temperature of the groove wall decreases, and the heat energy accumulates on the groove wall, forming an obvious heat-affected zone. When the scanning speed is faster, the cumulative temperature of the groove wall is lower, the laser energy distribution becomes uneven, and the overlapping area of ​​adjacent pulses decreases, resulting in incomplete ablation areas on the groove wall and poor ablation morphology. At the same time, it was found that the depth of ablation decreased significantly, from 49.7μm to 17.32μm, because the laser action time at any point was reduced, resulting in a decrease in the energy deposition at that point. Since the ablation depth mainly depends on the total amount of energy deposition, the increase in scanning speed will significantly reduce the ablation depth; and femtosecond laser ablation mainly removes materials through optical breakdown and high-temperature thermal effects. The depth is affected by energy deposition and heat penetration depth. At a slower scanning speed, the heat accumulation in the laser action area is more significant, which helps to increase the ablation depth. The width of the ablation did not change significantly, from 56.5μm to 44.1μm, because the ablation width is more affected by the laser focus spot size, the heat effect mainly propagates in the depth direction, and the width is mainly affected by the laser spot size and energy distribution, so the increase in scanning speed has a relatively small effect on the width.

[0063] Figure 5 (a) Figure 5 (b) Figure 5 (c) Figure 5(d) represents the ablation simulation of the NiCoCrAlY metal bonding layer under 30, 40, 50 and 60 cyclic scanning times, respectively. As the number of scans increases, the thermal accumulation temperature of the groove wall increases, which in turn causes thermal expansion and contraction, resulting in large thermal stress, which further causes defects. At the same time, it is found that the width of the groove does not change significantly. This is because the spot of the femtosecond laser is small, its energy is highly concentrated at the focus, and the energy density of the laser is relatively uniformly distributed in the horizontal direction. Due to the large thermal impedance in the depth direction, the heat is mainly conducted along the depth direction. In contrast, the heat diffusion in the horizontal direction is faster, so the groove width does not change significantly. As the number of scans increases, the groove depth changes greatly. This is because the energy density of the laser has a large gradient along the direction perpendicular to the material surface. The high peak power of the femtosecond laser can produce extremely high temperatures in an instant, causing the material to evaporate rapidly. This evaporation mainly occurs in the area of ​​the beam focus, and the material removal along the depth direction is more significant, resulting in obvious changes in the depth direction. The simulation results are consistent with the experimental results. The changes in the groove width and depth are mainly due to the combined effect of factors such as the energy distribution characteristics of the femtosecond laser, the heat conduction effect, the material removal mechanism, and the optical limitation.

[0064] Through simulation analysis, the temperature distribution and dynamics of energy exchange of the NiCoCrAlY metal bonding layer processed by femtosecond laser are obtained, the influence of different laser process parameters on the ablation of the material is predicted, and the three-dimensional morphology produced by the ablation is obtained. It has important applications in predicting and controlling the ablation morphology, providing a cost-effective way to explore the influence of different laser parameters on the processing results, which helps to guide parameter selection and process optimization.

[0065] Single factor ablation experiment

[0066] The present invention uses ablation experiments based on the ablation mechanism of femtosecond lasers and adopts the single factor principle of control variables on the basis of simulation result parameters to explore the influence of different laser ablation processing parameters, including laser energy density, scanning speed and number of cycle scanning, on material removal depth and surface quality. Based on the simulation analysis results of laser processing of NiCoCrAlY materials, the laser process parameters are optimized and determined by achieving the processing goals of no obvious heat-affected zone, no microcracks, no holes, and no molten droplets in the coating; and the determined laser process parameters are used to achieve femtosecond laser fine processing of the NiCoCrAlY metal bonding layer coating without thermal damage. The femtosecond laser processing system includes a femtosecond laser system and a three-axis displacement platform, and equipment such as Figure 6As shown, the femtosecond laser has a pulse width of 300fs-ps, a wavelength of 1030nm and a repetition rate of 25kHz-5000kHz. As shown in the figure, the optical route consists of a beam expander, a reflector, a CCD camera system for real-time monitoring and precise positioning of the workpiece, and a scanning galvanometer system for quickly and accurately directing the laser beam and controlling the scanning path and position of the laser beam on the workpiece. A field lens with a focal length of 100mm is used to focus the laser beam directly on the surface of the NiCoCrAlY coating, with a spot diameter of about 35μm and a focal depth of about 0.1mm.

[0067] Top view SEM images of NiCoCrAlY coatings ablated under different laser energy densities are shown in Figure 2. Figure 7 As shown, Figure 7 (a) Figure 7 (b) Figure 7 (c) Figure 7 (d) represents 1.948 J / cm 2 , 2.831J / cm 2 , 3.737J / cm 2 and 4.521 J / cm 2 The ablation experiment of NiCoCrAlY metal bonding layer under laser energy density is shown in Figure 2. Figure 7 (a) It can be seen that when the laser energy density is low, incomplete ablation areas appear in the grooves and irregular or rough textures are produced on the surface. This is because the laser does not provide enough energy to obtain a clear and smooth ablation surface. Figure 7 (b) The processing quality is good. It is a linear groove with very clear and smooth edges, and there is no obvious remelting layer and heat-affected zone. Since the laser ablation of NiCoCrAlY coating adopts the method of reciprocating scanning, the heat energy of the laser accumulates in the material. This heat accumulation will cause local overheating of the material, resulting in melting and resolidification in the ablation area. Figure 7 (c) and 7(d) show that with the increase of laser energy density, a large number of irregular protrusions and pores appear inside the groove. Such protrusions appear in the laser ablation process of different materials. Their formation depends largely on the surface tension and rapid solidification of the material. Such rapid solidification will generate stress inside the material, thereby forming cracks and voids in the molten material. At the same time, it can be observed that when the energy density is high, the material removal method is mainly phase explosion, the edge quality of the micro-groove is poor, and there is a significant heat-affected zone (HAZ).

[0068] The top view SEM images of the ablated NiCoCrAlY coating at different laser scanning speeds are shown in Figure 2. Figure 8 As shown, Figure 8 (a) Figure 8 (b) Figure 8 (c) Figure 8(d) represents the ablation of NiCoCrAlY metal bonding layer at laser scanning speeds of 600 mm / s, 800 mm / s, 1000 mm / s and 1200 mm / s, respectively. Figure 8 (a) It can be found that cracks, holes or remelting appear on the processed surface. These defects will reduce the smoothness and overall quality of the processed surface. The reason for the defects is that when the scanning speed is low, the action time of the laser per unit area increases, resulting in more heat accumulation on the material surface and its surrounding areas. Especially under the action of continuous or repeated pulses, the heat cannot be dissipated through heat conduction in time, resulting in heat accumulation in local areas. Due to heat accumulation, the heat affected zone (HAZ) near the processing area increases significantly. In this area, the material will undergo microstructural changes such as grain growth, phase change or stress concentration. Figure 8 (b) It can be found that the machined wall is smooth and the machined surface is uniform, which ensures the overall performance and appearance quality of the machined part. There is no obvious heat-affected zone, no microcracks, holes, molten droplets and other processing defects. Figure 8 (c) It can be found that when the scanning speed increases, the heat accumulation effect decreases, but because the laser's action time on the material surface is reduced, the processing depth of the material by a single laser pulse decreases, thereby reducing the overall material removal rate. Some incomplete ablation areas appear in the figure. This unevenness will affect the overall performance and appearance quality of the processed part. Figure 8 (d) It can be found that when the scanning speed is too high, the material removal rate is very low. High scanning speed means that the laser beam acts on a given area for a reduced time, resulting in less energy absorbed by the area. If the energy is not enough to reach the ablation threshold of the material, effective material removal cannot be achieved, especially on the wall or deep area. The wall area in the figure shows a higher surface roughness value, and the surface appears uneven, rough, with microscopic protrusions and depressions. For coatings or composite materials, the quality of the contact surface affects the adhesion and integrity of the interface. Poor processing quality may cause the coating to fall off or the interface to weaken. Although increasing the scanning speed can reduce heat accumulation and heat-affected zone, too high a speed will lead to a decrease in processing removal rate, reduced processing quality and uniformity, and reduced energy utilization efficiency. Therefore, when choosing an appropriate scanning speed, it is necessary to consider both avoiding thermal effects and ensuring processing effects and efficiency.

[0069] The top view SEM images of the ablated NiCoCrAlY coating under different laser scanning times are shown in Figure 2. Fig. 9 As shown by Fig. 9(a) It was found that insufficient scanning times resulted in poor quality of the ablated surface or features, resulting in rough surface and uneven morphology. Due to the inadequate ablation process, there was a clear boundary between the unablated area and the ablated area, and obvious pores were observed at the bottom of the groove. Fig. 9 (b) It can be clearly observed that as the ablation depth increases, the wall surface becomes smoother without obvious rough texture. The smooth surface means less thermal impact and finer material removal control. The depth of the groove is uniform in the entire processing area without obvious depth changes, which indicates that the energy distribution and material removal process are uniform and the processing size is accurate. However, too many scans will cause heat energy to accumulate in the ablation area, such as Fig. 9 (c) and Fig. 9 (d) It can be found that heat accumulation leads to the expansion of the heat-affected zone, affecting the microstructure and properties of the material, and causing stress concentration or microcracks.

[0070] S6. Determine laser process parameters and perform heat-damage-free femtosecond laser processing based on simulation and experimental results

[0071] According to the simulation results and experimental results, the laser process parameters were further optimized to 2.831-3.137J / cm 2 High-quality microstructure texture grooves were successfully prepared under the conditions of laser energy density of 2.831 J / cm 2 The best results are obtained when the laser energy density is 40, the number of scans is 40, and the laser scanning speed is 800 mm / s. Fig.10 As shown, Fig.10 (a) is a top view of the SEM morphology, with very clear and smooth edges, and no obvious remelting layer and heat-affected zone. This shows that the femtosecond laser has extremely high precision and control capabilities during the processing, and can form regular and smooth grooves on the NiCoCrAlY material. The inner wall of the groove is smooth and flawless, and no microcracks or molten droplets are observed, which further verifies the heat-free damage characteristics of femtosecond laser processing and achieves heat-free damage treatment of the coating. Fig.10(b) is a schematic diagram of the cross-section of the microstructure. The depth and shape of the groove can be clearly seen in the cross-section, and the cross-sectional morphology is regular with clear boundaries. This shows that the material removal during femtosecond laser processing is uniform, and there is no obvious heat-affected zone and microcracks. The bottom of the groove is smooth, the side walls are vertical, and there is no residue of molten material. This shows that the femtosecond laser can maintain extremely high processing accuracy at high energy density, while avoiding the common thermal effect problems in traditional laser processing. By optimizing the three parameters of laser energy density, scanning speed, and number of scans, a significant synergistic effect is achieved. Specifically, an appropriate laser energy density (2.831-3.137J / cm 2 ) ensures that the energy deposited by each pulse on the material surface is uniform, avoiding excessive or insufficient ablation; combined with a moderate scanning speed (800-1000mm / s), the material removal process is uniform and precise, preventing melting and uneven processing; and the optimized number of scans (40-45 times) ensures that the depth and morphology of the microstructure meet the expectations, avoiding excessive processing and surface damage. The synergistic effect of these three parameters not only reduces the generation of heat-affected zones, but also achieves uniform material removal and precise control of microstructures, ultimately significantly improving processing quality and efficiency, and demonstrating a significant synergy effect.

[0072] Schematic diagram of three-dimensional contour morphology Fig.11 shown. Fig.11 (a) shows the 3D morphology of the groove formed by femtosecond laser processing. It can be observed that the groove has a very clear outline, the groove edge is neat and smooth, and the groove bottom has a regular morphology. The 3D image further verifies the uniformity of material removal during femtosecond laser processing, with no obvious remelting layer and heat-affected zone, indicating that femtosecond laser has minimal thermal influence on the material during processing, and can achieve high-precision microstructure processing. Fig.11 (b) shows a cross-sectional profile showing the depth and width of the groove. The groove is about 30 μm deep and 50 μm wide. The cross-sectional profile is smooth and symmetrical, and the sidewalls are almost perpendicular to the bottom of the groove. Such a cross-sectional morphology shows that during femtosecond laser processing, the laser energy deposition is uniform and controlled, and the material removal process is stable and precise. No microcracks or holes were observed in the cross-sectional image, which further verifies that the femtosecond laser maintains extremely high processing accuracy at high energy density while avoiding common defects in traditional laser processing. Using 2.831-3.137 J / cm 2The laser energy density can ensure the ablation removal rate, optimize the oxidation degree, and ensure the quality of micro-grooves and surface accuracy. When the scanning times are 40-45 times, the material removal rate can be guaranteed and high-quality grooves can be obtained. Too many scanning times will cause the deposited material to undergo oxidation reaction to form oxides. When the laser scanning speed is 800-1000mm / s, the material removal rate is high, the processing wall is smooth, the processing surface is uniform, there is no obvious heat-affected zone and ablation heat accumulation, and fine processing of NiCoCrAlY coating without thermal damage is achieved.

[0073] Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A femtosecond laser processing method for NiCoCrAlY bonding layer microstructure, characterized in that: The steps include: S1. Establish the ablation model of NiCoCrAlY material processed by femtosecond laser; S2, heat source add-on for ablation model; S3, setting of boundary conditions; S4, simulation of ablated NiCoCrAlY metal bonding layer combined with dual-temperature equation; S5. Determine laser process parameters through simulation results and perform femtosecond laser processing without thermal damage.

2. The femtosecond laser processing method for NiCoCrAlY bonding layer microstructure according to claim 1, characterized in that: In step S1, numerical simulation software is used to model the bonding layer of the turbine NiCoCrAlY metal material. The ablation model is a three-dimensional geometric model with a size of 300μm×300μm×100μm in the xyz direction. An adaptive strategy is adopted for mesh division, and free tetrahedral mesh is used for division to adapt to complex geometric shapes and boundary conditions. A distributed mesh density is used in the z direction, specifically including: a fine mesh is used in the area close to the surface, i.e., 0-20μm, and the mesh density is gradually reduced in the depth direction, i.e., 20-100μm; a uniform mesh is used in the surface area, i.e., 0-300μm, in the x and y directions.

3. The femtosecond laser processing method for NiCoCrAlY bonding layer microstructure according to claim 1, characterized in that: In step S2, the heat source loading term adopts the transient physical field method, and the upper surface of the geometric model is used as the loading surface of the laser heat source. The laser beam is vertically incident on the surface and distributes its energy in the ablation area. On the plane, the heat source term adopts a two-dimensional Gaussian distribution, and in the depth direction, the heat source term adopts an exponential decay form; the laser energy distribution function S acting on the surface of the metal material is specifically expressed as follows: Where R represents the temperature-dependent interface reflectivity of the surface, F0 is the laser peak energy density, and τ p is the laser pulse width, t0 is the position of the first laser peak in the time domain, w0 is the pulse laser focus spot radius, and α(x, y, z, t) is the laser absorption coefficient.

4. The femtosecond laser processing method for NiCoCrAlY bonding layer microstructure according to claim 1, characterized in that: In step S3, in order to accurately simulate the boundary conditions of heat conduction during femtosecond laser ablation, each boundary surface of the model is set respectively. The boundaries and bottom surface of the model are set to a constant temperature of 300K, and the heat flux is zero, that is, no heat is dissipated outward through these surfaces; the boundary condition formula is expressed as follows: Among them, T e , T l They represent the transient temperatures of the electronic system and the lattice system respectively, k is the thermal conductivity, Q0 represents the heat source on the surface of the electronic system, and l represents the side length of the simulation model.

5. The femtosecond laser processing method for NiCoCrAlY bonding layer microstructure according to claim 1, characterized in that: In step S4, the specific steps include: S41. The dual-temperature equation is used to simulate the established femtosecond laser processing NiCoCrAlY material ablation model; S42. Using different femtosecond laser process parameters, i.e., different laser energy densities, laser scanning speeds, and different repeated scanning times, to simulate the ablation of the NiCoCrAlY metal bonding layer, the temporal and spatial distribution of the electron temperature inside the material, the temporal and spatial distribution of the lattice temperature inside the material, the energy exchange process between the electronic system and the lattice system and its influencing factors, and the overall thermal response behavior of the material under the action of the femtosecond laser pulse, including the heating, cooling, and thermal diffusion processes; S43. Through simulation analysis, the temperature distribution and energy exchange dynamics of the NiCoCrAlY metal bonding layer processed by femtosecond laser are obtained, the influence of different laser process parameters on the ablation of the material is predicted, and the three-dimensional morphology produced by the ablation is obtained.

6. The femtosecond laser processing method for NiCoCrAlY bonding layer microstructure according to claim 5, characterized in that: In step S41, the energy transfer between the electron and lattice systems is described by a two-temperature equation, accurately reflecting the thermal effect of the interaction between the femtosecond laser and the material; in the two-temperature equation, the electron system and the lattice system have different temperature fields, respectively, and the evolution of these two temperature fields is controlled by the following two coupled partial differential equations, and the control equations are expressed as follows: Among them, the subscripts e and l represent electrons and lattices respectively, C represents heat capacity, G is the electron-lattice coupling coefficient, and S represents the laser energy distribution function acting on the surface of the metal material.

7. The femtosecond laser processing method for NiCoCrAlY bonding layer microstructure according to claim 1, characterized in that: In step S5, based on the simulation analysis results of laser processing of NiCoCrAlY material, the laser process parameters are optimized and determined by achieving the processing purpose of having no obvious heat-affected zone, no microcracks, no holes, and no molten droplets in the coating; and the determined laser process parameters are used to achieve femtosecond laser fine processing of the NiCoCrAlY metal bonding layer coating without thermal damage.

8. The femtosecond laser processing method for NiCoCrAlY bonding layer microstructure according to claim 7, characterized in that: The determined laser process parameters specifically refer to: 2.831-3.137J / cm 2 The laser energy density is 800-1000mm / s, the laser scanning speed is 800-1000mm / s, and the laser cycle scanning times are 40-45 times.

9. The femtosecond laser processing method for NiCoCrAlY bonding layer microstructure according to claim 7, characterized in that: The determined laser process parameters specifically refer to: 2.831J / cm 2 The laser energy density is 800mm / s, the laser scanning speed is 800mm / s and the number of laser cycle scanning is 40 times.

Citation Information

Cited By

  • Array type high-energy laser countering unmanned aerial vehicle test method and device

    CN119198168A

  • A test method and device for array high-energy laser countermeasure against UAV

    CN119198168B

  • Quality control method and system suitable for laser surface treatment of valve workpiece

    CN119668225A

  • Trajectory optimization method and device for laser on-the-fly processing

    CN119758878A

  • Liquid metal bearing surface laser processing technological parameter simulation optimization method

    CN119849066A