Metal thin-wall structure with active cooling function and manufacturing method
Through the diffusion connection technology of prefabricated inner runner metal blank sheet and metal material, combined with fluid medium cooling, the problem of insufficient temperature resistance of traditional metal components is solved, efficient manufacturing of metal thin-walled components is achieved, and the temperature resistance performance of high-speed aircraft is improved and manufacturing efficiency.
Patent Information
- Application Number
- CN202411217722.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-11-01
AI Technical Summary
Traditional metal components are difficult to meet the high temperature resistance needs of high-speed aircraft. Ceramic materials are limited by the forming process and low plasticity properties in the manufacturing of large components. Materials such as high temperature alloys are high in density and difficult to promote due to high processing.
Prefabricated inner runner metal blank sheet material is used to create a metal thin-wall structure with active cooling function through metal material diffusion connection technology. The inner runner is passed into the fluid medium to improve the temperature resistance level.
It has achieved temperature resistance improvement of metal thin-walled components, extended service life and safety, broken through the bottleneck of the design and manufacturing of the cooling system in thin-walled components, and improved the integrity and consistency of blank sheet materials.
Smart Images

Figure CN118875663A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of material processing and manufacturing, and relates to an active cooling functional structure and a manufacturing method. Background Art
[0002] As the requirements for the running speed of vehicles are getting higher and higher, and the high flight speed makes the new generation of fighters have higher requirements for the flight speed, the high flight speed makes the aerodynamic skin surface of the fuselage produce high temperature due to high-speed friction, so more stringent requirements are put forward for the temperature resistance of the aircraft aerodynamic surface components. At present, traditional metal components are difficult to match the required temperature resistance level, and some high temperature resistance coatings need to be coated on their surfaces. However, the structure of the metal surface coating is essentially a combination of two structures, involving the bonding force between the two. In a complex and harsh service environment, the bonding layer between the two will be seriously affected, causing the bonding force to drop significantly, causing the heat-resistant coating to fall off, and destroying the heat resistance of the components. For this reason, some researchers directly use ceramics and other materials with higher temperature resistance to make structural parts, and have achieved good results in the field of component level and small components. However, due to the current forming process level and the low plasticity of ceramics, it is still limited in the field of manufacturing larger parts. In addition, some scholars have proposed the use of metals with higher temperature resistance, such as high-temperature alloys, tungsten and intermetallic compounds for manufacturing. Similarly, if this method is used, firstly, the density of the material itself is high, which will lead to a significant increase in the weight of the fighter; secondly, the material preparation is difficult, the cost is high, and the poor processing performance makes it difficult to promote and apply it in large and complex components. Therefore, it is urgent to find a low-cost and efficient manufacturing method suitable for the manufacture of large aerodynamic shape components to meet the manufacturing needs of high-speed aircraft. Summary of the invention
[0003] In view of the current situation that the temperature resistance of traditional metal thin-walled components mentioned above does not match the current development needs of high-speed aircraft, the present invention proposes a metal thin-walled structure and manufacturing method with active cooling function, which is achieved by adopting a process method of prefabricating an inner flow channel metal blank sheet and then forming an aerodynamic surface component configuration. The present invention adopts the diffusion bonding technology of metal materials, assembling the plates that have completed the flow channel manufacturing in advance and placing them in the diffusion bonding equipment to make a blank sheet with a prefabricated inner flow channel, and then placing the prefabricated blank sheet in the forming equipment to complete the manufacture of the thin-walled structure with active cooling function. The present invention realizes the manufacture of thin-walled components with inner flow channel structures, and the introduction of fluid medium into the inner flow channel improves the temperature resistance level of metal thin-walled components, which promotes the application of thin-walled components in high-speed aircraft.
[0004] In order to achieve the above purpose, the technical means adopted by the present invention are as follows:
[0005] Active cooling functional metal thin-wall structure, the active cooling functional metal thin-wall structure is an integrated structure, including a structural inner layer, a structural outer layer and a flow channel between the two layers through which a fluid medium with heat exchange properties can pass, the overall configuration characteristics meet the requirements of the aerodynamic shape characteristics of high-speed aircraft, and finally form an aircraft metal thin-wall skin structure with fluid medium flow heat exchange function;
[0006] The active cooling function is that during the use of the metal thin-walled structure, the outer surface of the outer layer of the structure rubs against the surrounding atmosphere and other media at high speed, and the surface temperature rises greatly, causing the metal thin-walled structure to fail. When a fluid medium is introduced into the flow channel of the metal thin-walled structure, the flow of the fluid medium takes away the heat generated by friction, so that the temperature of the metal surface is always below the failure temperature of the selected metal, thereby improving the service life and safety of the metal thin-walled component.
[0007] The inner layer and the outer layer of the structure are made of the same or different metal materials with high-temperature diffusion connection characteristics. The flow channel structure is located on the diffusion connection side surface of the outer layer of the structure and is manufactured by mechanical milling or chemical milling, while the inner layer of the structure is a metal sheet.
[0008] The flow channel structure is a plurality of flow channels arranged in parallel array, or distributed in a serpentine manner inside the metal thin-wall structure, which mainly depends on the allowable heat exchange efficiency η of the metal thin-wall structure with active cooling function and the fluid medium flow rate m required for the heat exchange efficiency. The surface of the flow channel structure is provided with a micro-nano structure with resistance reduction characteristics to reduce the resistance of the fluid medium when flowing in the flow channel;
[0009] The integrated configuration is a structural inner layer and a structural outer layer with a flow channel structure, the structural outer layer on the flow channel structure side is bonded inwardly with the structural inner layer, and then a blank required for manufacturing a metal thin-walled component with an inner flow channel structure is manufactured through a diffusion bonding process, and the blank is formed and manufactured in a component forming tool to complete the profile of the final component;
[0010] The present invention also provides a forming process for realizing the above-mentioned active cooling function thin-wall structure, characterized in that the steps are as follows:
[0011] Step 1: Forming the outer layer of the structure
[0012] 1.1 Preparation of structural outer layer materials
[0013] According to the structural features of the outer layer of the structure, a net size expansion figure is produced in the 3D drawing software. Based on the net size expansion figure, a margin is added around the net size expansion figure. The margin size is 100-150mm. The maximum outer dimension of the margin shape is determined as the cutting size of the raw materials used for manufacturing the outer layer of the structure, and the raw materials are prepared;
[0014] 1.2 Manufacturing of structural outer components
[0015] The prepared raw material is used with three positioning holes as the reference, and a concave structural feature of the flow channel is produced on the surface of the raw material according to the designed size and path of the flow channel by using a chemical milling process;
[0016] Step 2: Forming the inner layer of the structure
[0017] Preparation of structural inner layer materials and component manufacturing
[0018] The inner layer of the structure adopts the original sheet material configuration. Therefore, according to the structural characteristics of the inner layer of the structure, a net size development diagram is made in the 3D drawing software. Based on the net size development diagram, a margin is added to the circumference of the net size development diagram. The margin size is 100-150mm. The circumference contour size of the inner layer sheet material of the structure is required to be larger than the circumference contour size of the outer layer sheet material of the structure. The maximum outer contour size of the margin shape is determined as the blanking size of the raw material used for the inner layer of the structure, and the raw material preparation is completed;
[0019] Step 3: Blank sheet forming
[0020] 3.1 Preparation before diffusion bonding
[0021] Coat solder paste on the flow channel features of the outer plate particles of the structure, fit the plate surface of the inner raw material of the structure with the flow channel feature side of the outer plate material of the structure, and use laser welding method to seal the misaligned edges of the inner and outer peripheries of the structure to complete the sealing of the bonding surface of the inner and outer layers of the structure, and connect the ventilation pipe by welding at the inlet and outlet of the flow channel features;
[0022] 3.2 Diffusion bonding
[0023] The double-layer sheet to be welded after sealing welding is placed flatly in the diffusion mold and placed in the diffusion furnace as a whole with the diffusion mold to perform diffusion connection of the double-layer sheet. When the diffusion connection is about 2 / 3 of the cycle, argon gas is introduced into the ventilation pipe to ensure that the inner flow channel features are unobstructed, and finally the inner flow channel metal blank sheet preform is formed;
[0024] Step 4: Component Forming
[0025] The prefabricated inner flow channel metal blank sheet is placed in the hot forming tooling, and then put into the hot forming furnace again together with the hot forming tooling to achieve the final forming of the required shape of the component. Then, the laser cutting process is used to manufacture the component's outer contour according to the component's digital model, and finally the thin-walled structure with inner flow channel features is manufactured.
[0026] Beneficial effects of the present invention:
[0027] (1) A manufacturing method for thin-walled components with active cooling function is proposed, which breaks through the bottleneck of design and manufacturing of the cooling system inside the thin-walled components, enables the thin-walled components to realize cooling functionality, and can improve the temperature resistance level of the thin-walled components;
[0028] (2) The use of diffusion-connected prefabricated flow channel features in combination with hot forming technology to complete component manufacturing can effectively improve the integrity and consistency of the blank sheet;
[0029] (3) The blank sheet material with diffusion connection prefabricated flow channel features proposed in the present invention can be used for the manufacture of blank sheets for forming other thin-walled components such as superplastic forming, in addition to being used for hot forming thin-walled components proposed in the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 Schematic diagram of thin-wall structure with active cooling function;
[0031] Figure 2 Schematic diagram for determining the material cutting of the outer layer of the structure;
[0032] Figure 3 Schematic diagram of cutting materials for the inner layer of the structure;
[0033] Figure 4 Schematic diagram of the component structure before forming;
[0034] Figure 5 Schematic diagram of the inner flow channel metal blank preform.
[0035] In the figure: 1 is a thin-walled structure with active cooling function; 2 is the outer layer of the structure; 3 is the inner layer of the structure; 4 is the flow channel; 5 is the blanking contour for manufacturing the outer layer of the structure; 6 is the blanking contour for manufacturing the inner layer of the structure; 7 is the ventilation duct; 8 is the structure before the component profile is formed; 9 is the blank preform. DETAILED DESCRIPTION
[0036] The present invention is further described in detail below in conjunction with the accompanying drawings so that those skilled in the art can implement the invention with reference to the description.
[0037] Embodiment 1:
[0038] Active cooling functional metal thin-wall structure, the active cooling functional metal thin-wall structure is an integrated structure, including a structural inner layer 3, a structural outer layer 2, and a flow channel between the two layers through which a fluid medium with heat exchange properties can pass. The overall configuration characteristics meet the requirements of the aerodynamic shape characteristics of high-speed aircraft, and finally form an aircraft metal thin-wall skin structure with fluid medium flow heat exchange function;
[0039] The active cooling function is that when the metal thin-walled structure is in use, the outer surface of the outer layer 2 of the structure and the surrounding atmosphere and other media are subjected to high-speed friction, and the surface temperature rises greatly, causing the metal thin-walled structure to fail. When a fluid medium is introduced into the flow channel of the metal thin-walled structure, the flow of the fluid medium takes away the heat generated by friction, so that the temperature of the metal surface is always below the failure temperature of the selected metal, thereby improving the service life and safety of the metal thin-walled component.
[0040] The structural inner layer 3 and the structural outer layer 2 are made of the same or different metal materials with high-temperature diffusion connection characteristics. The flow channel structure is located on the diffusion connection side surface of the structural outer layer 2 and is manufactured by mechanical milling or chemical milling, while the structural inner layer 3 is a metal sheet.
[0041] The flow channel structure is a plurality of flow channels arranged in parallel array, or distributed in a serpentine manner inside the metal thin-wall structure, which mainly depends on the allowable heat exchange efficiency η of the metal thin-wall structure with active cooling function and the fluid medium flow rate m required for the heat exchange efficiency. The surface of the flow channel structure is provided with a micro-nano structure with resistance reduction characteristics to reduce the resistance of the fluid medium when flowing in the flow channel;
[0042] The integrated configuration is a structural inner layer 3 and a structural outer layer 2 with a flow channel structure, and the structural outer layer 2 on the flow channel structure side is bonded inwardly to the structural inner layer 3, and then a blank required for manufacturing a metal thin-walled component with an inner flow channel structure is formed by a diffusion bonding process, and the blank is formed and manufactured in a component forming tool to complete the profile of the final component;
[0043] The present invention also provides a forming process for realizing the above-mentioned active cooling function thin-wall structure, characterized in that the steps are as follows:
[0044] Step 1: Forming the outer layer of the structure 2
[0045] 1.1 Structural outer layer 2 material preparation
[0046] According to the structural features of the outer layer 2 of the structure, a net size development graphic is produced in a three-dimensional drawing software. Based on the net size development graphic, a margin is added to the circumference of the net size development graphic. The margin size is 100 to 150 mm. The maximum outer dimension of the margin shape is determined as the blanking size of the raw materials used for manufacturing the outer layer 2 of the structure, and the raw materials are prepared;
[0047] 1.2 Manufacturing of structural outer layer 2 components
[0048] The prepared raw material is used with three positioning holes as the reference, and a concave structural feature of the flow channel is produced on the surface of the raw material according to the designed size and path of the flow channel by using a chemical milling process;
[0049] Step 2: Forming the inner layer 3
[0050] Structural inner layer 3 material preparation and component manufacturing
[0051] The inner layer 3 of the structure adopts the original sheet material configuration. Therefore, according to the structural characteristics of the inner layer 3 of the structure, a net size development diagram is made in the three-dimensional drawing software. Based on the net size development diagram, a margin is added to the circumference of the net size development diagram. The margin size is 100-150mm. It is required that the circumference contour size of the sheet material of the inner layer 3 of the structure is larger than the circumference contour size of the sheet material of the outer layer 2 of the structure. The maximum outer contour size of the margin shape is determined as the blanking size of the raw material used for manufacturing the inner layer 3 of the structure, and the raw material preparation is completed;
[0052] Step 3: Blank sheet forming
[0053] 3.1 Preparation before diffusion bonding
[0054] Coat solder paste on the flow channel feature of the plate particles of the outer layer 2 of the structure, fit the plate surface of the raw material of the inner layer 3 of the structure with the flow channel feature side of the plate material of the outer layer 2 of the structure, and use laser welding method to seal the staggered edges of the inner layer 3 of the structure and the outer layer 2 of the structure to complete the sealing of the bonding surface of the inner layer 3 of the structure and the outer layer 2 of the structure, and connect the ventilation pipe by welding at the inlet and outlet of the flow channel feature;
[0055] 3.2 Diffusion bonding
[0056] The double-layer sheet to be welded after the sealing welding is placed flatly in the diffusion mold and placed in the diffusion furnace as a whole with the diffusion mold to perform diffusion connection of the double-layer sheet. When the diffusion connection is performed for about 2 / 3 of the cycle, argon gas is introduced into the ventilation pipe 7 to ensure that the inner flow channel feature is unobstructed, and finally the inner flow channel metal blank sheet preform is formed;
[0057] Step 4: Component Forming
[0058] The prefabricated inner flow channel metal blank sheet is placed in the hot forming tooling, and then put into the hot forming furnace again together with the hot forming tooling to achieve the final forming of the required shape of the component. Then, the laser cutting process is used to manufacture the component's outer contour according to the component's digital model, and finally the thin-walled structure with inner flow channel features is manufactured.
[0059] Embodiment 2:
[0060] The active cooling function thin-walled structure 1 is characterized by a structure outer layer 2, a structure inner layer 3, and a flow channel 4 between the two layers on the structure outer layer for passing cooling water. The manufacturing process is as follows:
[0061] Step 1: Open the digital model of the structural outer layer 2 of the component to be manufactured in the three-dimensional drawing software, and use the unfolding function in the software to make the unfolded graphics of the structural outer layer 2, and expand the outline of the unfolded graphics of the structural outer layer 2 as a reference to increase the margin of 150mm to form the blanking outline 5 for manufacturing the structural outer layer 2, and then perform laser cutting and blanking, and use the chemical milling process to remove the flow channel 4 on the structural outer layer 2 to remove the flow channel material characteristics;
[0062] Step 2: Open the digital model of the inner layer 3 of the component structure to be manufactured in the 3D drawing software, and use the unfolding function in the software to make the unfolded graphics of the inner layer 3 of the structure, and expand the outline of the unfolded graphics of the inner layer 3 of the structure as a reference to increase the margin of 100mm to form the blanking outline 6 of the inner layer 3 of the structure, and then perform laser cutting;
[0063] Step 3: Apply solder stop on the flow channel feature of the outer layer of the junction, cover the inner layer 3 sheet material of the structure to the upper side of the solder stop coating side of the outer layer 2 of the structure, adjust the spatial position of the inner layer 3 sheet material of the structure between the outer layer 2 of the structure, so that the inner layer 3 sheet material of the structure is in the middle of the outer layer 2 sheet material of the structure, and form a staggered edge feature on the circumference, and the staggered edge amount of each side is not less than 20mm, and use laser welding technology to seal the inner layer 3 and the outer layer 2 sheet materials of the structure in the form of fillet joint along the staggered edge position of the circumference, and weld the ventilation pipe 7 at the inlet and outlet of the flow channel feature to form a component profile pre-forming structure 8 that is fixed on all sides and has a gap inside before diffusion connection;
[0064] Step 4: Place the welded parts to be diffused into the diffusion bonding tooling, and place the whole parts into the diffusion furnace for diffusion bonding. During the diffusion bonding process, fill the vent pipe at the inlet of the flow channel feature with argon gas every 20 to 30 minutes to detect the smoothness of the flow channel feature, and finally complete the diffusion bonding of the inner layer 3 of the structure and the outer layer 2 of the structure to form the inner flow channel metal.
[0065] Step 5: Place the preform 9 into the forming tool, and place it into the forming furnace together with the forming tool as a whole, and finally form the part profile. Finally, use the laser cutting method to remove the excess of the component, and thus complete the manufacture of the thin-walled component with active cooling function.
Claims
1. Active cooling functional metal thin-wall structure, characterized by: The active cooling functional metal thin-wall structure is an integrated structure, comprising a structural inner layer (3), a structural outer layer (2), and a flow channel between the two layers through which a fluid medium with heat exchange properties can flow; The structural inner layer (3) and the structural outer layer (2) are both made of the same or different metal materials with high-temperature diffusion bonding characteristics, the flow channel structure is located on the diffusion bonding side surface of the structural outer layer (2), and the structural inner layer (3) is a metal plate; The flow channel structure is a plurality of flow channels arranged in parallel array, or distributed in a serpentine shape inside the metal thin-wall structure; The integrated structure comprises a structural inner layer (3) and a structural outer layer (2) with a flow channel structure. The structural outer layer (2) on the flow channel structure side is bonded inwardly to the structural inner layer (3), and then a blank required for manufacturing a metal thin-walled component with an internal flow channel structure is manufactured through a diffusion bonding process. The blank is then formed into a final component profile in a component forming tool.
2. The active cooling functional metal thin-wall structure according to claim 1, characterized in that: The surface of the flow channel structure is provided with a micro-nano structure having a resistance-reducing property.
3. The active cooling functional metal thin-wall structure according to claim 1 or 2, characterized in that: The flow channel structure is manufactured by mechanical milling or chemical milling.
4. The method for manufacturing an active cooling functional metal thin-walled structure according to any one of claims 1 to 3, characterized in that: Here are the steps: Step 1: Forming the outer layer of the structure 1.1 Structural outer layer (2) Material preparation According to the structural features of the outer layer (2) of the structure, a net size expansion figure is produced in a three-dimensional drawing software, and a margin is added around the net size expansion figure based on the net size expansion figure, and the margin size is 100 to 150 mm. The maximum outer contour size of the margin shape is determined as the cutting size of the raw materials used for manufacturing the outer layer (2) of the structure, and the raw materials are prepared; 1.2 Structural outer layer (2) Component manufacturing The prepared raw material is used with three positioning holes as the reference, and a concave structural feature of the flow channel is produced on the surface of the raw material according to the designed size and path of the flow channel by using a chemical milling process; Step 2: Forming the inner layer of the structure (3) Structural inner layer (3) Material preparation and component manufacturing The structural inner layer (3) adopts the original sheet material configuration, and a net size development diagram is produced in a three-dimensional drawing software according to the structural characteristics of the structural inner layer (3). A margin is added around the net size development diagram based on the net size development diagram, and the margin size is 100 to 150 mm. The maximum outer contour size of the margin shape is determined as the blanking size of the raw material used for manufacturing the structural inner layer (3), and the raw material preparation is completed; Step 3: Blank sheet forming 3.1 Preparation before diffusion bonding A solder stop is applied to the flow channel feature of the plate particles of the outer layer (2) of the structure, the plate surface of the raw material of the inner layer (3) of the structure is fitted with the flow channel feature side of the plate material of the outer layer (2) of the structure, and a laser welding method is used to perform sealing welding at the misaligned edges of the circumference of the inner layer (3) of the structure and the outer layer (2) of the structure, so as to complete the sealing of the fitting surface of the inner layer (3) of the structure and the outer layer (2) of the structure; 3.2 Diffusion bonding The double-layer sheet to be welded after the sealing welding is placed flatly in the diffusion mold and the diffusion mold is placed as a whole in the diffusion furnace to perform diffusion connection of the double-layer sheet; Step 4: Component Forming The prefabricated inner flow channel metal blank sheet is placed in the hot forming tooling, and then put into the hot forming furnace again together with the hot forming tooling to achieve the final forming of the required shape of the component. Then, the laser cutting process is used to manufacture the component's outer contour according to the component's digital model, and finally the thin-walled structure with inner flow channel features is manufactured.
5. The method for manufacturing an active cooling functional metal thin-wall structure according to claim 4, characterized in that: In the step 2, the circumferential contour size of the plate material of the inner layer (3) of the structure is larger than the circumferential contour size of the plate material of the outer layer (2) of the structure.
6. The method for manufacturing an active cooling functional metal thin-walled structure according to claim 4 or 5, characterized in that: In the step 3.1, after the sealing of the fitting surfaces of the inner structure layer (3) and the outer structure layer (2) is completed, the ventilation pipes are connected at the inlet and outlet of the flow channel feature by welding.
7. The method for manufacturing an active cooling functional metal thin-walled structure according to claim 4 or 5, characterized in that: In the step 3.2, when the diffusion bonding is carried out for 2 / 3 of the cycle, argon gas is introduced into the ventilation pipe (7) to form an inner flow channel metal blank sheet material preform.
8. The method for manufacturing an active cooling functional metal thin-wall structure according to claim 3, characterized in that: In the step 3.2, when the diffusion bonding is carried out for 2 / 3 of the cycle, argon gas is introduced into the ventilation pipe (7) to form an inner flow channel metal blank sheet material preform.
Citation Information
Patent Citations
Superplastic forming / diffusion bonding forming method for heat-resistant titanium alloy envelope
CN106271439A
Heat treatment method of thin-wall SPF / DB hollow structure
CN109207890A
Preparation method for changing titanium alloy into variable-wall thick hollow active cooling cabin
CN110480279A
Preparing method of aluminum alloy light-weight active cooling structure skin
CN110539138A
Method and device for processing skin with active cooling channel
CN113001127A