Production process of silica gel integral plate without adhesive

By using uniform leveling mixing of the central layer containing glass fiber and the external silicone board in the silicone board process, the problem of uneven mixing of adhesives under high temperature and high pressure is solved, and the mechanical properties and elongation of break of the silicone board are improved. .

CN118876471APending Publication Date: 2024-11-01ANHUI LIANGCHEN SILICON MATERIAL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410843334.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing clamped silicone plates have inconsistent melting points of adhesive and silicone in high temperature and high pressure environments, resulting in uneven mixing, affecting the mechanical properties and elongation of break.

Method used

A silicone plate containing glass fiber is used as the central layer, and a silicone plate containing no adhesive is formed by preparing in advance and re-melting in the process, and re-melting is carried out in a uniform leveling manner, combining foaming and vulcanization treatment.

Benefits of technology

The hardness, tensile strength, thermal stability and ozone resistance of the silicone plate are improved, while the elongation of break is increased, ensuring the uniform performance of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of silica gel plate processing, in particular to a production process of an adhesive-free silica gel integral plate, which specifically comprises the following steps: (1) proportionally taking silicone rubber, glass fiber, a foaming agent and a vulcanizing agent, mixing, and melting to form a central rubber compound; uniformly plastifying the central rubber compound, then calendaring into a silica gel sheet, finally, synchronously foaming and vulcanizing the silica gel sheet to obtain a thick central clamping plate, and cutting the thick central clamping plate into a thin plate with the thickness of 1-3mm to obtain a central clamping plate; and (2) taking silicone rubber, a foaming agent, a plasticizer and a vulcanizing agent in proportion, mixing, melting to form a rubber compound, extruding the rubber compound into a mold, placing the central clamping plate in the middle layer of the rubber compound, and finally foaming and vulcanizing the rubber compound and the central clamping plate in the mold. Experiments prove that the high-hardness and high-ozone-resistance silica gel plate has hardness, tensile strength, thermal stability and ozone resistance which are consistent with those of a cloth-sandwiched silica gel plate, and also has higher elongation at break.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of silica gel plate processing, in particular to a production process of a silica gel integral plate without adhesive. Background Art

[0002] Silicone has the characteristics of organic polymer elastomers and the wide high and low temperature adaptability of inorganic substances. Silicone products have become the preferred material in military aerospace, medical, automotive, construction and other fields.

[0003] In the prior art, silicone sheets are usually processed in different ways depending on the usage scenarios, including common ordinary silicone integral sheets and cloth-inserted silicone sheets, etc. The silicone integral sheets are produced by silicone mixing-extrusion molding-vulcanization treatment, while the cloth-inserted silicone sheets are produced by placing glass fiber cloth in the mold during extrusion molding, so that the extruded silicone sheets will have glass fiber cloth sandwiched in the silicone sheets, achieving the technical effect of improving physical and chemical properties. However, since adhesives such as water-based resins are used in the production of glass fiber cloth, the external high temperature and high pressure environment will melt the adhesive during extrusion molding and vulcanization treatment, and the melting points of the adhesive and silicone are inconsistent. The heating and cooling process will cause the molten adhesive and silicone to mix, and the adhesive will be subjected to external forces such as extrusion during the mixing process, which will cause the adhesive to be mixed evenly at different locations in the center of the silicone sheet, and ultimately cause the mechanical properties of the finished product of the cloth-inserted silicone sheet to change after cooling. Summary of the invention

[0004] In order to solve the problems raised in the above background technology, the present invention provides a production process of a silicone integral plate without adhesive.

[0005] To achieve the above object, the present invention provides the following technical solutions: A production process of a silicone integral plate without adhesive is as follows: (1) 100-150 parts by mass of silicone rubber, 10-20 parts by mass of glass fiber, 2-4 parts by mass of foaming agent and 1-3 parts by mass of vulcanizing agent are mixed and melted to form a core rubber compound; the core rubber compound is plasticized and evenly rolled into a silicone sheet; finally, the silicone sheet is subjected to simultaneous foaming and vulcanization in a normal pressure environment at a temperature of 130-150° C. for 30-50 minutes to obtain a rough core plywood; the rough core plywood is cut into thin plates with a thickness of 1-3 mm to obtain a core plywood; (2) 100-150 parts by mass of silicone rubber, 2-4 parts by mass of foaming agent, 1-3 parts by mass of plasticizer and 1-3 parts by mass of vulcanizer are mixed and melted to form a rubber compound, which is extruded into a mold and the center plywood is placed in the middle layer thereof. Finally, the rubber compound and the center plywood in the mold are foamed and vulcanized for 20-40 minutes to obtain the obtained product.

[0006] Furthermore, the silicone rubber is a combination of one or more of methyl vinyl silicone rubber, methyl phenyl vinyl silicone rubber, fluorosilicone rubber and silicon nitrogen rubber.

[0007] Furthermore, the glass fiber is alkali-free glass fiber.

[0008] Furthermore, the vulcanizing agent is an alkylphenol-formaldehyde resin or an epoxy resin.

[0009] Compared with the prior art, the present invention has the following beneficial effects: The present invention adopts a pre-made silicone plate containing glass fibers as the central layer, thereby solving the problem of low elongation at break caused by directly using glass fiber cloth as the central layer of the cloth-inserted silicone plate. Since water-based resin and other adhesives are used in the production of glass fiber cloth, the adhesive will be melted by the external high temperature and high pressure environment during extrusion molding and vulcanization treatment. The melting points of the adhesive and the silicone are inconsistent, and the molten adhesive and the silicone are mixed in the heating and cooling process. The adhesive is subjected to external forces such as extrusion during the mixing process, which will cause the mixing uniformity of the adhesive at various places in the center of the silicone plate to be inconsistent, and finally cause the cloth-inserted silicone plate to have a low elongation at break after cooling. Since the central layer of the present invention adopts a silicone plate containing glass fibers, it can be uniformly leveled and mixed with the external silicone plate when it is melted again after being used as a sandwich plate, and the influence of subsequent foaming and vulcanization on the silicone plate of the central layer is also minimized. In this way, the final product has the same hardness, tensile strength, thermal stability and ozone resistance as the cloth-inserted silicone plate, and also has a higher elongation at break. DETAILED DESCRIPTION Example 1

[0010] A production process of a silicone integral plate without adhesive is as follows: (1) 100 parts of silicone rubber, 10 parts of glass fiber, 2 parts of foaming agent and 1 part of vulcanizing agent are mixed and melted to form a core rubber compound; the core rubber compound is plasticized and evenly rolled into a silicone sheet; finally, the silicone sheet is subjected to simultaneous foaming and vulcanization in a normal pressure environment at a temperature of 130° C. for 30 minutes to obtain a rough core plywood; the rough core plywood is cut into a sheet with a thickness of 1 mm to obtain a core plywood; (2) 100 parts of silicone rubber, 2 parts of foaming agent, 1 part of plasticizer and 1 part of vulcanizer are mixed and melted to form a rubber compound, which is extruded into a mold and the center plywood is placed in the middle layer. Finally, the rubber compound and the center plywood in the mold are foamed and vulcanized for 20 minutes to obtain a rubber compound.

[0011] Furthermore, the silicone rubber is a combination of one or more of methyl vinyl silicone rubber, methyl phenyl vinyl silicone rubber, fluorosilicone rubber and silicon nitrogen rubber.

[0012] Furthermore, the glass fiber is alkali-free glass fiber.

[0013] Furthermore, the vulcanizing agent is an alkylphenol-formaldehyde resin or an epoxy resin. Example 2

[0014] A production process of a silicone integral plate without adhesive is as follows: (1) 150 parts by mass of silicone rubber, 20 parts by mass of glass fiber, 4 parts by mass of foaming agent and 3 parts by mass of vulcanizing agent are mixed and melted to form a core rubber compound; the core rubber compound is plasticized and evenly rolled into a silicone sheet; and finally the silicone sheet is subjected to simultaneous foaming and vulcanization at a temperature of 150° C. and a normal pressure environment for 50 minutes to obtain a rough core plywood; the rough core plywood is cut into a sheet with a thickness of 3 mm to obtain a core plywood; (2) 150 parts of silicone rubber, 4 parts of foaming agent, 3 parts of plasticizer and 3 parts of vulcanizer are mixed and melted to form a rubber compound, which is extruded into a mold and the center plywood is placed in the middle layer. Finally, the rubber compound and the center plywood in the mold are foamed and vulcanized for 40 minutes to obtain a rubber compound.

[0015] Furthermore, the silicone rubber is a combination of one or more of methyl vinyl silicone rubber, methyl phenyl vinyl silicone rubber, fluorosilicone rubber and silicon nitrogen rubber.

[0016] Furthermore, the glass fiber is alkali-free glass fiber.

[0017] Furthermore, the vulcanizing agent is an alkylphenol-formaldehyde resin or an epoxy resin. Example 3

[0018] A production process of a silicone integral plate without adhesive is as follows: (1) 120 parts by mass of silicone rubber, 15 parts by mass of glass fiber, 3 parts by mass of foaming agent and 2 parts by mass of vulcanizing agent are mixed and melted to form a core rubber compound; the core rubber compound is plasticized and evenly rolled into a silicone sheet; and finally the silicone sheet is subjected to simultaneous foaming and vulcanization at a temperature of 140° C. and a normal pressure environment for 40 minutes to obtain a rough core plywood; the rough core plywood is cut into a sheet with a thickness of 2 mm to obtain a core plywood; (2) 120 parts of silicone rubber, 3 parts of foaming agent, 2 parts of plasticizer and 2 parts of vulcanizer are mixed and melted to form a rubber compound, which is extruded into a mold and the center plywood is placed in the middle layer. Finally, the rubber compound and the center plywood in the mold are foamed and vulcanized for 30 minutes to obtain a rubber compound.

[0019] Furthermore, the silicone rubber is a combination of one or more of methyl vinyl silicone rubber, methyl phenyl vinyl silicone rubber, fluorosilicone rubber and silicon nitrogen rubber.

[0020] Furthermore, the glass fiber is alkali-free glass fiber.

[0021] Furthermore, the vulcanizing agent is an alkylphenol-formaldehyde resin or an epoxy resin.

[0022] Control group 1 The manufacturing process of the ordinary silicone integral plate without interlayer is the same as that of the silicone plate obtained in step (2) without adding the central sandwich plate.

[0023] Control group 2 The existing silicone splint uses glass fiber cloth as the central layer.

[0024] The five groups of silicone plates were cut into strips of 100mm*10mm*10mm, and their hardness, tensile strength, elongation at break, thermal stability temperature range and ozone resistance were tested respectively. The ozone resistance test method is to place them in 50±5pphm, 10℃ ozone for 70h and observe whether there are obvious cracks on the surface. The results are as follows:

[0025] It can be seen from the above table that the silicone plate prepared by the present invention is consistent with the silicone plate sandwiched with glass fiber cloth on the market in terms of hardness, tensile strength, thermal stability and ozone resistance, and at the same time solves the problem of low fracture productivity of the silicone plate sandwiched with glass fiber cloth, and the product quality is better and the market competitiveness is stronger.

[0026] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.

[0027] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A production process for a silicone monolithic plate without adhesive, characterized in that: The details are as follows: (1) 100-150 parts by mass of silicone rubber, 10-20 parts by mass of glass fiber, 2-4 parts by mass of foaming agent and 1-3 parts by mass of vulcanizing agent are mixed and melted to form a core rubber compound; the core rubber compound is plasticized and evenly rolled into a silicone sheet; finally, the silicone sheet is subjected to simultaneous foaming and vulcanization in a normal pressure environment at a temperature of 130-150° C. for 30-50 minutes to obtain a rough core plywood; the rough core plywood is cut into thin plates with a thickness of 1-3 mm to obtain a core plywood; (2) 100-150 parts by mass of silicone rubber, 2-4 parts by mass of foaming agent, 1-3 parts by mass of plasticizer and 1-3 parts by mass of vulcanizer are mixed and melted to form a rubber compound, which is extruded into a mold and the center plywood is placed in the middle layer thereof. Finally, the rubber compound and the center plywood in the mold are foamed and vulcanized for 20-40 minutes to obtain the obtained product.

2. The production process of a silicone integral plate without adhesive according to claim 1, characterized in that: Step (1) is preferably performed by mixing 120 parts of silicone rubber, 15 parts of glass fiber, 3 parts of foaming agent and 2 parts of vulcanizing agent by weight and then melting them to form a core rubber compound; the core rubber compound is plasticized evenly and then rolled into a silicone sheet; finally, the silicone sheet is subjected to simultaneous foaming and vulcanization in a normal pressure environment at a temperature of 140° C. for 40 minutes to obtain a rough core plywood; the rough core plywood is cut into thin plates with a thickness of 2 mm to obtain a core plywood.

3. The production process of a silicone integral plate without adhesive according to claim 1, characterized in that: Preferably, step (2) comprises the following steps: taking 120 parts of silicone rubber, 3 parts of foaming agent, 2 parts of plasticizer and 2 parts of vulcanizer, by weight, mixing and melting to form a rubber mixture; extruding the rubber mixture into a mold, placing the center plywood in the middle layer thereof, and finally foaming and vulcanizing the rubber mixture and the center plywood in the mold for 30 minutes.

4. The production process of a silicone monolithic plate without adhesive according to any one of claims 1 to 3, characterized in that: The silicone rubber is a combination of one or more of methyl vinyl silicone rubber, methyl phenyl vinyl silicone rubber, fluorosilicone rubber and silicon nitrogen rubber.

5. The production process of a silicone integral plate without adhesive according to any one of claims 1 to 3, characterized in that: The glass fiber is alkali-free glass fiber.

6. The production process of a silicone monolithic plate without adhesive according to any one of claims 1 to 3, characterized in that: The vulcanizing agent is an alkylphenol-formaldehyde resin or an epoxy resin.