Composite fiber felt and composite board for automobile door interior decoration board and preparation method and application of composite fiber felt and composite board
Through the needle-punching consolidation of glass fiber and polypropylene fiber and high-pressure hot plate pressing process, low-weight, high-strength, and low shrinkage composite boards were prepared, which solved the problem of high weight and easy deformation of traditional automotive door interior decorative board materials. The problem of natural fibers that are prone to mold meets the automotive industry's demand for high-performance materials and is environmentally friendly and recyclable.
Patent Information
- Application Number
- CN202411353203.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-26
- Publication Date
- 2024-11-19
AI Technical Summary
The materials of traditional automotive door interior decorative panels are high in weight and are prone to shrinkage and deformation. Natural fiber-reinforced thermoplastics are prone to mold and lack of rigidity, and the supply chain is unstable, which affects the mechanical properties and user experience of the car.
The composite fiber felt is made by needle-punching and consolidating glass fibers in a certain proportion, and the composite sheet is made by combining the high-pressure hot plate pressing process to ensure that the proportion of inorganic fibers is not lower than that of thermoplastic fibers to improve the rigidity and deformation resistance of the material.
It realizes composite boards with low weight, high strength, low shrinkage, mildew and recycling, which improves the mechanical properties and use stability of the interior decorative panels of the car doors and reduces production costs.
Smart Images

Figure BDA0005062879700000081 
Figure BDA0005062879700000101 
Figure BDA0005062879700000111
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of automobile door interior decoration board preparation, and in particular to a composite fiber felt and a composite board for automobile door interior decoration board, and a preparation method and application thereof. Background Art
[0002] Car door interior panels are an important part of the car, and their quality and performance directly affect the overall appearance and user experience of the car. With the development of the new energy vehicle industry, the performance requirements for car door interior panels are getting higher and higher. They not only need to have a good appearance, but also excellent mechanical properties and dimensional stability, and also have a significant weight reduction effect to meet the potential demands of mileage and endurance.
[0003] Traditional automobile door interior trim panels are currently mainly injection molded parts, and the materials are mainly thermoplastic materials such as polypropylene.
[0004] Composite sheet is a new type of material that is made of two or more materials of different properties through physical or chemical methods. It has the advantages of light weight, high strength, corrosion resistance, sound insulation, heat insulation, etc. It has been gradually applied to the fields of automobile door interior decoration panels in recent years. A pressed part molded from natural fiber reinforced thermoplastic plastics, such as hemp fiber reinforced polypropylene material. Patent CN100591549C describes a component for automotive interior products with a multi-layer structure, in which thermoplastic fibers as a substrate are mixed with thermoplastic organic fibers and natural fibers as reinforcing fibers in various mixing ratios, and a multi-layer structure is formed by the fiber mixture, and the multi-layer structure is compressed and expanded in a continuous composite sheet manufacturing device. This lightweight composite sheet contains environmentally friendly natural fibers, has excellent noise elimination and absorption, heat insulation, durability, light weight, recyclability and high specific stiffness properties, and can be used for automotive interior parts such as glove boxes, door linings, roof linings and seat backs, as well as industrial materials.
[0005] However, these materials have their own problems:
[0006] Although thermoplastic injection molded parts allow a high degree of freedom in construction and design, they are relatively heavy and prone to thermal deformation. In addition, the thermoplastic material must be heated to above its melting point during the injection molding process and injection molded under sufficient pressure. Therefore, the production process consumes a lot of energy and is prone to defective parts.
[0007] Composite sheets are prone to deformation after heating and molding, which not only affects the appearance of the product, but may also affect the performance of the product, causing abnormal noise and loose opening and closing of the door. In addition, although natural fiber reinforced thermoplastic pressed parts only need to be baked through and then directly cold molded to shape, natural fibers are prone to mold under different conditions of use, and natural fibers are coarse in diameter and are not easily penetrated by thermoplastic materials, which can easily cause problems such as cracking after molding and insufficient rigidity of the whole piece. Natural fibers rely on imports, there are supply bottlenecks, and the quality of hemp fibers cannot be guaranteed to be consistent due to weather restrictions.
[0008] In addition, the car door interior decorative panel is the main decorative part inside the door panel. Speaker-related equipment will be added on it later. During the operation of the vehicle, if it can have a better sound-absorbing effect, it can bring a better driving experience to the driver and passengers. Summary of the invention
[0009] In order to solve the above problems, the present invention provides a composite fiber felt, a composite board and a preparation method and application thereof for automobile door interior decorative panels, which solve the problems of high gram weight and easy shrinkage and deformation of injection-molded parts of automobile door interior decorative panels; mildew and poor strength of pressed parts containing natural fibers.
[0010] In order to achieve the above object, the present invention provides the following technical solutions:
[0011] The present invention provides a composite fiber felt for an automobile door interior decorative panel, wherein the raw materials of the composite fiber felt include glass fiber and polypropylene fiber;
[0012] The mass ratio of the glass fiber to the polypropylene fiber is 4-6:4-6;
[0013] The fiber length of the glass fiber is 25 to 100 mm and the diameter is 15 to 20 μm;
[0014] The polypropylene fiber has a fiber length of 25 to 100 mm, a fineness of 5 to 9D, a breaking strength of 18 to 36 N, a breaking tenacity of 2 to 4 CN, an elongation of 150 to 250%, and a melt index of 15 to 50 g / 10 min.
[0015] Preferably, the mass ratio of the glass fiber to the polypropylene fiber is 4:6.
[0016] Preferably, the melt index of the polypropylene fiber is 30 g / 10 min.
[0017] The present invention also provides a method for preparing the composite fiber mat described in the above technical solution, comprising the following steps: sequentially opening, combing, web laying and needle punching the glass fiber and the polypropylene fiber to obtain the composite fiber mat;
[0018] The carding conditions include: feed rate of 600-900 kg / h, bulk density of each layer of felt material of 0.1-0.6 g / cm 3 ;
[0019] The conditions and parameters of the web laying include: a width of 1000 to 3300 mm, 6 to 100 web laying layers, and a web laying speed of 0.5 to 200 m / min;
[0020] The acupuncture condition parameters include: the distance between the needle loom plates is 16 to 20 mm, the needle depth is 7 to 12 mm, and the needle density is 40 to 100 needles / cm 2 .
[0021] The present invention also provides a composite board for automobile door interior decoration, which comprises, from bottom to top, an exterior facing layer, an adhesive film, the composite fiber felt described in the above technical solution, an adhesive film and an interior facing layer.
[0022] Preferably, the thickness of the composite plate is 3 to 4 mm;
[0023] The thickness of the interior surface layer is 1.0-1.2 mm, the material is PET fiber fabric, the elongation at break is greater than 75%, the shrinkage is 8-15%, and the weight is 80 g / m 2 ;
[0024] The thickness of the film is 0.032-0.034 mm, the material is a perforated polypropylene film, the pore size is 0.5-1 mm, and the weight is 30 g / m 2 ;
[0025] The composite fiber felt has a thickness of 8.0 to 11.0 mm and a gram weight of 1140 g / m 2 ;
[0026] The thickness of the outer facing layer is 1.0-1.2 mm, the material is polyester fiber fabric, the elongation at break is greater than 75%, the shrinkage is 8-15%, and the weight is 80 g / m 2 .
[0027] The present invention also provides a method for preparing the composite board described in the above technical solution, comprising the following steps: placing the outer facing layer, adhesive film, composite fiber felt, adhesive film and inner facing layer in sequence and pressurizing them to obtain a composite board.
[0028] Preferably, the pressurizing conditions include: temperature of 200-220° C., pressure of 5-8 MPa, hot plate gap of 0, and pressure holding for 30 seconds.
[0029] The present invention also provides the use of the composite board described in the above technical solution in improving the mechanical properties of the interior decorative board of an automobile door.
[0030] Preferably, the mechanical properties include one or more of tensile strength, tensile modulus, tensile yield strain, flexural strength, flexural modulus and flexural stiffness.
[0031] The present invention forms a composite fiber felt by consolidating thermoplastic fibers (polypropylene fibers) and inorganic fibers (glass fibers) in a certain proportion through needle punching, thereby avoiding the problem of easy deformation caused by high thermoplastic components, maintaining the cohesion between the two fibers in the composite fiber felt, thereby effectively improving the continuity of stress transfer of the resin inside the material, and improving the fracture strength and elongation at break of the thermoplastic lightweight composite board. In the subsequent process, the felt and other auxiliary materials are pressed into a board by hot plate pressing under high pressure. The inorganic fibers in the composite fiber felt maintain the proportion of long fibers, and the thermoplastic fibers are fully melted and impregnated with the inorganic fibers under high temperature and high pressure, so that the pressed board can maintain good rigidity at low gram weight. Therefore, this reinforced LWRT material used for automotive door interior decorative panels has the characteristics of low gram weight and high strength, low shrinkage and low deformation, no mildew and can be recycled.
[0032] Beneficial effects of the present invention:
[0033] 1. Low weight and high strength: The present invention presses the composite fiber felt and other auxiliary materials into a board by hot plate pressing under high pressure. The inorganic fiber in the composite fiber felt maintains the proportion of long fiber. The thermoplastic fiber fully melts and impregnates the inorganic fiber under high temperature and high pressure, so that the pressed board can maintain good rigidity at low weight. The traditional production process of door panels is injection molding, and the density of injection molding is generally 1.03-1.08g / cm 3 The material density of the board material after producing door panels is generally 0.85-0.93 g / cm 3 , compared with traditional processes, the weight can be reduced by 20%.
[0034] 2. Excellent formability: The present invention consolidates the composite fiber felt, thermoplastic fiber and inorganic fiber in a certain proportion by needle punching to form the composite fiber felt, thereby avoiding the problem of high shrinkage and easy deformation caused by high thermoplastic component, maintaining the cohesion between the two fibers in the composite fiber felt, thereby effectively improving the stress transfer continuity of the resin inside the material, improving the breaking strength and breaking elongation of the thermoplastic lightweight composite board, and being suitable for the deep forming requirements of automobile door interior panels.
[0035] 3. Low shrinkage and low deformation: The functional layers of the composite board described in the present invention: composite fiber felt, exterior facing layer, interior facing layer, all maintain a consistent shrinkage rate, so that the composite board has a good fit with the mold after heating and molding; and the structural design in which the proportion of inorganic fiber is not lower than that of thermoplastic fiber makes the composite board not easy to deform after heating and molding.
[0036] 4. No mildew and can be recycled: The composite board of the present invention is made of environmentally friendly materials, is non-toxic and odorless, will not mildew, and can be recycled and recycled, meeting environmental protection requirements. DETAILED DESCRIPTION
[0037] The present invention provides a composite fiber mat for automobile door interior decoration panels, wherein the raw materials of the composite fiber mat include glass fiber and polypropylene fiber; the mass ratio of the glass fiber to the polypropylene fiber is 4-6:4-6; the fiber length of the glass fiber is 25-100 mm, and the diameter is 15-20 μm; the fiber length of the polypropylene fiber is 25-100 mm, the fineness is 5-9D, the breaking strength is 18-36N, the breaking strength is 2-4CN, the elongation is 150-250%, and the melt index is 15-50 g / 10 min. In the present invention, the mass ratio of the glass fiber to the polypropylene fiber is preferably 4:6. In the present invention, the melt index of the polypropylene fiber is preferably 30 g / 10 min. The present invention has no special limitation on the sources of the glass fiber and the polypropylene fiber, and conventional commercially available products can be used. For example, the glass fiber is preferably EDR17-2400-360H produced by China Jushi Group, and the polypropylene fiber is preferably lightweight GMT-specific polypropylene staple fiber 8538B produced by Jiangsu Haibang New Materials Co., Ltd.
[0038] In the present invention, the composite fiber felt is a composite fiber felt obtained by blending thermoplastic fiber (polypropylene fiber) as a bonding matrix and inorganic fiber (glass fiber) as a reinforcing material.
[0039] In the present invention, the composite fiber felt is mainly a composite fiber felt made by blending 40-60% thermoplastic fibers and 50-60% inorganic fibers. The proportion of inorganic fibers contained therein is not lower than the proportion of thermoplastic fibers, so that the composite board is not easily deformed after heating and molding. If the proportion of thermoplastic fibers is too high, the composite board is prone to shrinkage and deformation after heating and molding; if the proportion of thermoplastic fibers is too low, after the composite fiber felt and other auxiliary materials are pressed into a composite board, the internal inorganic fibers cannot be well combined with the thermoplastic fibers, resulting in poor tensile properties of the board, and the composite board is prone to tearing after heating and molding.
[0040] The present invention also provides a method for preparing the composite fiber felt described in the above technical solution, comprising the following steps: opening, combing, laying and needle punching the glass fiber and polypropylene fiber in sequence to obtain a composite fiber felt; the combing condition parameters include: a feed rate of 600 to 900 kg / h, a bulk density of each layer of felt material of 0.1 to 0.6 g / cm 3The conditions and parameters of the web laying include: the width is 1000-3300mm, the number of web laying layers is 6-100 layers, and the web laying speed is 0.5-200m / min; the conditions and parameters of the acupuncture include: the distance between the needle punching machine plates is 16-20mm, the needle depth is 7-12mm, and the needle density is 40-100 needle punches / cm 2 .
[0041] The present invention also provides a composite board for automobile door interior decoration, which comprises, from bottom to top, an exterior facing layer, an adhesive film, the composite fiber felt described in the above technical solution, an adhesive film and an interior facing layer. In the present invention, the thickness of the composite board is preferably 3 to 4 mm.
[0042] In the present invention, the thickness of the interior surface layer is preferably 1.0-1.2 mm, the material is preferably PET fiber fabric, preferably prepared by white polyester fiber blended needle punching process, with a breaking elongation greater than 75%, a shrinkage rate of 8-15%, and a gram weight of 80 g / m 2 The white polyester fiber is preferably from Yangzhou Tianfulong Group, with a specification of 5dtex*51. In the present invention, the performance parameters of the interior surface layer and the exterior surface layer are consistent, ensuring the consistent shrinkage rate of the composite board during heating and baking, and the white color makes it easy to identify the area of the colored injection molded parts when adding injection molded parts to the interior surface, which plays a fool-proof effect.
[0043] In the present invention, the thickness of the film is preferably 0.032-0.034 mm, the material is a perforated polypropylene film, the pore size is preferably 0.5-1 mm, and the weight is 30 g / m 2 In the present invention, the perforated polypropylene film facilitates the air permeability of the composite board and is well bonded to the composite fiber felt and the inner and outer facing layers.
[0044] In the present invention, the thickness of the composite fiber felt is preferably 8.0 to 11.0 mm, and the gram weight is 1140 g / m 2 .
[0045] In the present invention, the thickness of the outer facing layer is preferably 1.0-1.2 mm, and the material is preferably polyester fiber fabric, preferably prepared by a black, white and gray three-color polyester fiber blended needle punching process, with a breaking elongation greater than 75%, a shrinkage rate of 8-15%, and a gram weight of 80 g / m 2 In the present invention, the outer facing layer with high elongation at break does not break at the deep forming part during the heating and molding process of the composite board, and the black, white and gray colors make the appearance of the surface video effect soft and smooth.
[0046] The present invention also provides a method for preparing the composite board described in the above technical solution, comprising the following steps: placing the outer facing layer, adhesive film, composite fiber felt, adhesive film and inner facing layer in sequence and pressurizing them to obtain a composite board.
[0047] In the present invention, the pressurizing conditions preferably include: temperature of 200-220° C., pressure of 5-8 MPa, hot plate gap of 0, and pressure holding for 30 seconds.
[0048] The present invention also provides the use of the composite sheet material described in the above technical solution in improving the mechanical properties of the interior decorative panel of an automobile door. In the present invention, the mechanical properties preferably include one or more of tensile strength, tensile modulus, tensile yield strain, bending strength, bending modulus and bending stiffness.
[0049] In order to further illustrate the present invention, the present invention is described in detail below in conjunction with embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0050] Example 1
[0051] A method for preparing a composite plate for an automobile door interior decorative plate, comprising the following steps:
[0052] Step 1: Prepare the ingredients:
[0053] Glass fiber and polypropylene fiber are selected as the main raw materials, among which glass fiber is mainly short and medium-length fiber with a fiber length of 50mm and a diameter of 17μm; polypropylene fiber is mainly short and medium-length fiber with a fiber length of 51mm, a fineness of 8D, and a melt index of 30g / 10min. The mass ratio of these two fibers is 50%:50%.
[0054] Step 2: Felt making by non-woven needle punching process:
[0055] The prepared glass fiber and polypropylene fiber are put into an opening machine for opening, and then the opened fibers are mixed and input into a carding machine for carding, and then the carded fibers are put into a web laying machine for web laying, and finally the web laying fibers are put into a needle punching machine for needle punching to obtain a composite fiber felt.
[0056] The feeding rate of the cotton feeding box in the mixing area is 600kg / h, and the bulk density of each layer of felt is 0.12g / cm 3 During the web laying process, the width is 2400mm, the number of web laying layers is 36, and the web laying speed range is 100m / min; the needle loom plate distance is 20mm, the needle depth is 9mm, and the needle density is 65 needles / cm 2 .
[0057] Step 3: Felt board making:
[0058] The interior surface layer, film, composite fiber felt, film, and exterior surface layer are placed on the continuous composite board manufacturing unwinding table in sequence. The interior surface layer is PET fiber fabric, which is made by needle punching process of black, white and gray polyester fiber blending, with elongation at break ≥75%, shrinkage 8-15%, and gram weight 80g / m 2 The film is a perforated polypropylene film with a pore size of 0.5-1mm and a gram weight of 30g / m 2 Composite fiber felt weight: 1140g / m 2 The outer surface layer is polyester fiber fabric, which is made by white polyester fiber blended needle punching process. The elongation at break of the fabric is ≥75%, the shrinkage is 8-15%, and the weight is 80g / m 2 .
[0059] The hot plate of the equipment is heated to 200℃, all materials enter the hot plate and are pressurized to 5MPa, the gap between the hot plates is 0, and the pressure is maintained for 30S to form a composite plate. The plate thickness is 4.0mm and the gram weight is 1350g / m 2 .
[0060] Step 4: Cutting: The prepared composite board is finally cut into the required size.
[0061] Example 2
[0062] A method for preparing a composite plate for an automobile door interior decorative plate, comprising the following steps:
[0063] Step 1: Prepare the ingredients:
[0064] Glass fiber and polypropylene fiber are selected as the main raw materials, among which glass fiber is mainly short and medium-length fiber with a fiber length of 50mm and a diameter of 17μm; polypropylene fiber is mainly short and medium-length fiber with a fiber length of 51mm, a fineness of 8D, and a melt index of 30g / 10min. The mass ratio of these two fibers is 50%:50%.
[0065] Step 2: Felt making by non-woven needle punching process:
[0066] The prepared glass fiber and polypropylene fiber are put into an opener for opening, and then the opened fibers are put into a carding machine for combing, and then the carded fibers are put into a web laying machine for web laying, and finally the web laying fibers are put into a needle punching machine for needle punching to obtain a composite fiber felt.
[0067] The feeding rate of the cotton feeding box in the mixing area is 600kg / h, and the bulk density of each layer of felt is 0.12g / cm 3 During the web laying process, the width is 2400mm, the number of web laying layers is 36, and the web laying speed range is 100m / min; the needle loom plate distance is 20mm, the needle depth is 9mm, and the needle density is 65 needles / cm 2.
[0068] Step 3: Felt board making:
[0069] The interior surface layer, film, composite fiber felt, film, and exterior surface layer are placed on the continuous composite board manufacturing unwinding table in sequence. The interior surface layer is PET fiber fabric, which is made by needle punching process of black, white and gray polyester fiber blending. The fabric has a breaking elongation of ≥75%, a shrinkage of 8-15%, and a gram weight of 80g / m 2 The film is a perforated polypropylene film with a pore size of 0.5-1mm and a gram weight of 30g / m 2 Composite fiber felt weight: 1140g / m 2 The outer surface layer is made of polyester fiber fabric using white polyester fiber blended needle punching technology. The elongation at break of the fabric is ≥75%, the shrinkage is 8-15%, and the weight is 80g / m 2 .
[0070] The hot plate is heated to 220℃, all materials enter the hot plate and are pressurized to 5MPa, the gap between the hot plates is 0, and the pressure is maintained for 30S to form a composite plate. The plate thickness is 3.5mm and the gram weight is 1350g / m 2 .
[0071] Step 4: Cutting: The prepared composite board is finally cut into the required size.
[0072] Example 3
[0073] A method for preparing a composite plate for an automobile door interior decorative plate, comprising the following steps:
[0074] Step 1: Prepare the ingredients:
[0075] Glass fiber and polypropylene fiber are selected as the main raw materials, among which glass fiber is mainly short and medium-length fiber with a fiber length of 50mm and a diameter of 17μm; polypropylene fiber is mainly short and medium-length fiber with a fiber length of 51mm, a fineness of 8D, and a melt index of 30g / 10min. The mass ratio of these two fibers is 50%:50%.
[0076] Step 2: Felt making by non-woven needle punching process:
[0077] The prepared glass fiber and polypropylene fiber are put into an opener for opening, and then the opened fibers are put into a carding machine for combing, and then the carded fibers are put into a web laying machine for web laying, and finally the web laying fibers are put into a needle punching machine for needle punching to obtain a composite fiber felt.
[0078] The feeding rate of the cotton feeding box in the mixing area is 600kg / h, and the bulk density of each layer of felt is 0.12g / cm 3During the web laying process, the width is 2400mm, the number of web laying layers is 36, and the web laying speed range is 100m / min; the needle loom plate distance is 20mm, the needle depth is 9mm, and the needle density is 65 needles / cm 2 .
[0079] Step 3: Felt board making:
[0080] The interior surface layer, film, composite fiber felt, film, and exterior surface layer are placed on the continuous composite board manufacturing unwinding table in sequence. The interior surface layer is PET fiber fabric, which is made by needle punching process of black, white and gray polyester fiber blending. The fabric has a breaking elongation of ≥75%, a shrinkage of 8-15%, and a gram weight of 80g / m 2 The film is a perforated polypropylene film with a pore size of 0.5-1mm and a gram weight of 30g / m 2 Composite fiber felt weight: 1140g / m 2 The outer surface layer is made of polyester fiber fabric using white polyester fiber blended needle punching technology. The elongation at break of the fabric is ≥75%, the shrinkage is 8-15%, and the weight is 80g / m 2 .
[0081] The hot plate of the equipment is heated to 220℃, all materials enter the hot plate and are pressurized to 8MPa, the gap between the hot plates is 0, and the pressure is maintained for 30S to form a composite plate. The plate thickness is 3.0mm and the gram weight is 1350g / m 2 .
[0082] Step 4: Cutting: The prepared composite board is finally cut into the required size.
[0083] Table 1 Test data of Examples 1-3
[0084]
[0085] Note: MD indicates the machine production output direction, and CD indicates the direction perpendicular to the machine production output direction.
[0086] It can be seen from the test data that increasing the temperature and pressure to thin the sheet can improve the mechanical properties of the sheet. However, when the temperature reaches 235°C and the pressure reaches 10MPa, on the one hand, the PP resin will overflow due to increased fluidity, and the resin content of the core layer will decrease. On the other hand, the PP resin will decompose due to high temperature, and the resin content of the core layer will also decrease. The bonding strength between PP resin and glass fiber will be reduced, and the mechanical properties of the sheet will decrease instead.
[0087] Example 4
[0088] A method for preparing a composite plate for an automobile door interior decorative plate, comprising the following steps:
[0089] Step 1: Prepare the ingredients:
[0090] Glass fiber and polypropylene fiber are selected as the main raw materials, among which glass fiber is mainly short and medium-length fiber with a fiber length of 50mm and a diameter of 17μm; polypropylene fiber is mainly short and medium-length fiber with a fiber length of 51mm, a fineness of 8D, and a melt index of 15g / 10min. The mass ratio of these two fibers is 50%:50%.
[0091] Step 2: Felt making by non-woven needle punching process:
[0092] The prepared glass fiber and polypropylene fiber are put into an opener for opening, and then the opened fibers are put into a carding machine for combing, and then the carded fibers are put into a web laying machine for web laying, and finally the web laying fibers are put into a needle punching machine for needle punching to obtain a composite fiber felt.
[0093] The feeding rate of the cotton feeding box in the mixing area is 600kg / h, and the bulk density of each layer of felt is 0.12g / cm 3 During the web laying process, the width is 2400mm, the number of web laying layers is 36, and the web laying speed range is 100m / min; the needle loom plate distance is 20mm, the needle depth is 9mm, and the needle density is 65 needles / cm 2 .
[0094] Step 3: Felt board making:
[0095] The interior surface layer, film, composite fiber felt, film, and exterior surface layer are placed on the continuous composite board manufacturing unwinding table in sequence. The interior surface layer is PET fiber fabric, which is made by needle punching process of black, white and gray polyester fiber blending. The fabric has a breaking elongation of ≥75%, a shrinkage of 8-15%, and a gram weight of 80g / m 2 The film is a perforated polypropylene film with a pore size of 0.5-1mm and a gram weight of 30g / m 2 Composite fiber felt weight: 1140g / m 2 The outer surface layer is made of polyester fiber fabric using white polyester fiber blended needle punching technology. The elongation at break of the fabric is ≥75%, the shrinkage is 8-15%, and the weight is 80g / m 2 .
[0096] The hot plate of the equipment is heated to 220℃, and all materials enter the hot plate and are pressurized to 5MPa. The gap between the hot plates is 0, and the pressure is maintained for 30S to form a composite plate. The plate thickness is 3.5mm and the gram weight is 1350g / m 2 .
[0097] Step 4: Cutting: The prepared composite board is finally cut into the required size.
[0098] Example 5
[0099] A method for preparing a composite plate for an automobile door interior decorative plate, comprising the following steps:
[0100] Step 1: Prepare the ingredients:
[0101] Glass fiber and polypropylene fiber are selected as the main raw materials, among which glass fiber is mainly short and medium-length fiber with a fiber length of 50mm and a diameter of 17μm; polypropylene fiber is mainly short and medium-length fiber with a fiber length of 51mm, a fineness of 8D, and a melt index of 50g / 10min. The mass ratio of these two fibers is 50%:50%.
[0102] Step 2: Felt making by non-woven needle punching process:
[0103] The prepared glass fiber and polypropylene fiber are put into an opener for opening, and then the opened fibers are put into a carding machine for combing, and then the carded fibers are put into a web laying machine for web laying, and finally the web laying fibers are put into a needle punching machine for needle punching to obtain a composite fiber felt.
[0104] The feeding rate of the cotton feeding box in the mixing area is 600kg / h, and the bulk density of each layer of felt is 0.12g / cm 3 During the web laying process, the width is 2400mm, the number of web laying layers is 36, and the web laying speed range is 100m / min; the needle loom plate distance is 20mm, the needle depth is 9mm, and the needle density is 65 needles / cm 2 .
[0105] Step 3: Felt board making:
[0106] The interior surface layer, film, composite fiber felt, film, and exterior surface layer are placed on the continuous composite board manufacturing unwinding table in sequence. The interior surface layer is PET fiber fabric, which is made by needle punching process of black, white and gray polyester fiber blending. The fabric has a breaking elongation of ≥75%, a shrinkage of 8-15%, and a gram weight of 80g / m 2 The film is a perforated polypropylene film with a pore size of 0.5-1mm and a gram weight of 30g / m 2 Composite fiber felt weight: 1140g / m 2 The outer surface layer is made of polyester fiber fabric using white polyester fiber blended needle punching technology. The elongation at break of the fabric is ≥75%, the shrinkage is 8-15%, and the weight is 80g / m 2 .
[0107] The hot plate of the equipment is heated to 220℃, and all materials enter the hot plate and are pressurized to 5MPa. The gap between the hot plates is 0, and the pressure is maintained for 30S to form a composite plate. The plate thickness is 3.5mm and the gram weight is 1350g / m 2 .
[0108] Step 4: Cutting: The prepared composite board is finally cut into the required size.
[0109] Table 2 Test data of embodiment 2 / 4 / 5
[0110]
[0111]
[0112] Note: MD indicates the machine production output direction, and CD indicates the direction perpendicular to the machine production output direction.
[0113] It can be seen from the test data that the influence trend of the melt index of polypropylene fiber on the board is as follows: when the melt index of polypropylene increases from 15g / 10min to 30g / 10min, the mechanical properties are significantly improved; when it increases from 30g / 10min to 50g / 10min, the improvement of mechanical properties slows down.
[0114] Example 6
[0115] A method for preparing a composite plate for an automobile door interior decorative plate, comprising the following steps:
[0116] Step 1: Prepare the ingredients:
[0117] Glass fiber and polypropylene fiber are selected as the main raw materials, among which glass fiber is mainly short and medium-length fiber with a fiber length of 50mm and a diameter of 17μm; polypropylene fiber is mainly short and medium-length fiber with a fiber length of 51mm, a fineness of 8D, and a melt index of 30g / 10min. The mass ratio of these two fibers is 40%:60%.
[0118] Step 2: Making felt through non-woven needle punching process.
[0119] The prepared glass fiber and polypropylene fiber are put into an opener for opening, and then the opened fibers are put into a carding machine for combing, and then the carded fibers are put into a web laying machine for web laying, and finally the web laying fibers are put into a needle punching machine for needle punching to obtain a composite fiber felt.
[0120] The feeding rate of the cotton feeding box in the mixing area is 600kg / h, and the bulk density of each layer of felt is 0.12g / cm 3 During the web laying process, the width is 2400mm, the number of web laying layers is 36, and the web laying speed range is 100m / min; the needle loom plate distance is 20mm, the needle depth is 9mm, and the needle density is 65 needles / cm 2 .
[0121] Step 3: Felt board making:
[0122] The interior surface layer, film, composite fiber felt, film, and exterior surface layer are placed on the continuous composite board manufacturing unwinding table in sequence. The interior surface layer is PET fiber fabric, which is made by needle punching process of black, white and gray polyester fiber blending. The fabric has a breaking elongation of ≥75%, a shrinkage of 8-15%, and a gram weight of 80g / m 2 The film is a perforated polypropylene film with a pore size of 0.5-1mm and a gram weight of 30g / m 2 Composite fiber felt weight: 1140g / m 2 The outer surface layer is made of polyester fiber fabric using white polyester fiber blended needle punching technology. The elongation at break of the fabric is ≥75%, the shrinkage is 8-15%, and the weight is 80g / m 2 .
[0123] The hot plate of the equipment is heated to 220℃, and all materials enter the hot plate and are pressurized to 5MPa. The gap between the hot plates is 0, and the pressure is maintained for 30S to form a composite plate. The plate thickness is 3.5mm and the gram weight is 1350g / m 2 .
[0124] Step 4: Cutting: The prepared composite board is finally cut into the required size.
[0125] Example 7
[0126] A method for preparing a composite plate for an automobile door interior decorative plate, comprising the following steps:
[0127] Step 1: Prepare the ingredients:
[0128] Glass fiber and polypropylene fiber are selected as the main raw materials, among which glass fiber is mainly short and medium-length fiber with a fiber length of 50mm and a diameter of 17μm; polypropylene fiber is mainly short and medium-length fiber with a fiber length of 51mm, a fineness of 8D, and a melt index of 30g / 10min. The mass ratio of these two fibers is 60%:40%.
[0129] Step 2: Felt making by non-woven needle punching process:
[0130] The prepared glass fiber and polypropylene fiber are put into an opener for opening, and then the opened fibers are put into a carding machine for combing, and then the carded fibers are put into a web laying machine for web laying, and finally the web laying fibers are put into a needle punching machine for needle punching to obtain a composite fiber felt.
[0131] The feeding rate of the cotton feeding box in the mixing area is 600kg / h, and the bulk density of each layer of felt is 0.12g / cm 3 During the web laying process, the width is 2400mm, the number of web laying layers is 36, and the web laying speed range is 100m / min; the needle loom plate distance is 20mm, the needle depth is 9mm, and the needle density is 65 needles / cm2 .
[0132] Step 3: Felt board making:
[0133] The interior surface layer, film, composite fiber felt, film, and exterior surface layer are placed on the continuous composite board manufacturing unwinding table in sequence. The interior surface layer is PET fiber fabric, which is made by needle punching process of black, white and gray polyester fiber blending. The fabric has a breaking elongation of ≥75%, a shrinkage of 8-15%, and a gram weight of 80g / m 2 The film is a perforated polypropylene film with a pore size of 0.5-1mm and a gram weight of 30g / m2. The composite fiber felt has a gram weight of 1140g / m 2 The outer surface layer is made of polyester fiber fabric using white polyester fiber blended needle punching technology. The elongation at break of the fabric is ≥75%, the shrinkage is 8-15%, and the weight is 80g / m 2 .
[0134] The hot plate of the equipment is heated to 220℃, and all materials enter the hot plate and are pressurized to 5MPa. The gap between the hot plates is 0, and the pressure is maintained for 30S to form a composite plate. The plate thickness is 3.5mm and the gram weight is 1350g / m 2 .
[0135] Step 4: Cutting: The prepared composite board is finally cut into the required size.
[0136] Table 3 Test data of embodiment 2 / 6 / 7
[0137]
[0138]
[0139] Note: MD indicates the machine production output direction, and CD indicates the direction perpendicular to the machine production output direction.
[0140] It can be seen from the test data that the mechanical properties of the glass fiber to polypropylene fiber ratio decreases as the glass fiber ratio increases.
[0141] Comparative Example 1
[0142] A method for preparing a composite plate for an automobile door interior decorative plate, comprising the following steps:
[0143] Step 1: Prepare the ingredients:
[0144] Hemp fiber and polypropylene fiber are selected as the main raw materials, among which hemp fiber is mainly short and medium-length fiber with a fiber length of 80-100mm and a diameter of 50μm; polypropylene fiber is mainly short and medium-length fiber with a fiber length of 51mm, a fineness of 8D, and a melt index of 30g / 10min. The feed weight ratio of glass fiber to polypropylene fiber is 50%:50%.
[0145] Step 2: Felt making by non-woven needle punching process:
[0146] The prepared hemp fiber and polypropylene fiber are put into an opener for opening, and then the opened fibers are put into a carding machine for combing, and then the carded fibers are put into a web laying machine for web laying, and finally the web laying fibers are put into a needle punching machine for needle punching to obtain a composite fiber felt.
[0147] The feeding rate of the cotton feeding box in the mixing area is 600kg / h, and the bulk density of each layer of felt is 0.15g / cm 3 During the web laying process, the width range is between 2400mm, the number of web laying layers ranges to 36 layers, and the web laying speed ranges to 100m / min; the needle loom plate distance is 18mm, the needle depth is 9mm, and the needle density is 65 needles / cm 2 .
[0148] Step 3: Felt board making:
[0149] The hot plate of the equipment is heated to 220℃, the felt is placed in the hot plate and pressurized to 5MPa, the gap between the hot plates is 0, and the pressure is maintained for 30S to form a composite plate. The plate thickness is 3.5mm and the gram weight is 1140g / m 2 .
[0150] Step 4: Cutting: The prepared composite board is finally cut into the required size.
[0151] Table 4 Test data of Example 2 and Comparative Example 1
[0152]
[0153] Note: MD indicates the machine production output direction, and CD indicates the direction perpendicular to the machine production output direction.
[0154] The test data shows that the mechanical properties of boards made of a combination of hemp fiber and polypropylene are weaker than those of a combination of glass fiber and polypropylene. In addition, the natural hygroscopicity of plant fibers causes their water content to be relatively high, making them more susceptible to mildew.
[0155] Due to the advanced nature of the technical solution, it can be widely used in application fields such as automobile manufacturing, environmental protection material research and development, and architectural decoration. First of all, the composite board of the present invention has the advantages of low gram weight and high strength, excellent formability, high shrinkage and low deformation, and no mildew and recyclability, which can greatly improve the performance of automobile door interior decoration panels and meet the high standards of the automobile industry for automobile door interior decoration panels. Secondly, in the preparation process of the composite board of the present invention, no organic solvents are used, and the composite board can also be recycled and reused, which is in line with the current development trend of green environmental protection and helps to promote the development of the environmental protection materials industry. Finally, the composite board of the present invention can also be widely used in the field of architectural decoration, such as interior decoration, outdoor billboards, public facilities decoration, etc., to meet people's demand for high-quality decorative materials.
[0156] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A composite fiber felt for automobile door interior decoration panel, characterized in that: The raw materials of the composite fiber felt include glass fiber and polypropylene fiber; The mass ratio of the glass fiber to the polypropylene fiber is 4-6:4-6; The fiber length of the glass fiber is 25 to 100 mm and the diameter is 15 to 20 μm; The polypropylene fiber has a fiber length of 25 to 100 mm, a fineness of 5 to 9D, a breaking strength of 18 to 36 N, a breaking tenacity of 2 to 4 CN, an elongation of 150 to 250%, and a melt index of 15 to 50 g / 10 min.
2. The composite fiber mat according to claim 1, characterized in that: The mass ratio of the glass fiber to the polypropylene fiber is 4:
6.
3. The composite fiber mat according to claim 1, characterized in that: The melt index of the polypropylene fiber is 30 g / 10 min.
4. A method for preparing the composite fiber felt according to any one of claims 1 to 3, characterized in that: The method comprises the following steps: sequentially opening, combing, web laying and needle punching the glass fiber and the polypropylene fiber to obtain a composite fiber mat; The carding conditions include: feed rate of 600-900 kg / h, bulk density of each layer of felt material of 0.1-0.6 g / cm 3 ; The conditions and parameters of the web laying include: a width of 1000 to 3300 mm, a number of web laying layers of 6 to 100, and a web laying speed of 0.5 to 200 m / min; The acupuncture condition parameters include: the distance between the needle loom plates is 16 to 20 mm, the needle depth is 7 to 12 mm, and the needle density is 40 to 100 needles / cm 2 .
5. A composite board for automobile door interior decoration, characterized in that: The invention comprises, from bottom to top, an outer facing layer, an adhesive film, the composite fiber felt according to any one of claims 1 to 6, an adhesive film and an inner facing layer.
6. The composite sheet material according to claim 5, characterized in that: The thickness of the composite plate is 3 to 4 mm; The thickness of the interior surface layer is 1.0-1.2 mm, the material is PET fiber fabric, the elongation at break is greater than 75%, the shrinkage is 8-15%, and the weight is 80 g / m 2 ; The thickness of the film is 0.032-0.034 mm, the material is a perforated polypropylene film, the pore size is 0.5-1 mm, and the weight is 30 g / m 2 ; The composite fiber felt has a thickness of 8.0 to 11.0 mm and a gram weight of 1140 g / m 2 ; The thickness of the outer facing layer is 1.0-1.2 mm, the material is polyester fiber fabric, the elongation at break is greater than 75%, the shrinkage is 8-15%, and the weight is 80 g / m 2 .
7. A method for preparing the composite board according to claim 6, characterized in that: The following steps are involved: The exterior facing layer, adhesive film, composite fiber felt, adhesive film and interior facing layer are sequentially placed and pressurized to obtain a composite board.
8. The preparation method according to claim 7, characterized in that: The pressurizing conditions include: temperature of 200-220° C., pressure of 5-8 MPa, hot plate gap of 0, and pressure holding for 30 seconds.
9. Use of the composite sheet material according to claim 5 or 6 in improving the mechanical properties of automobile door interior decorative panels.
10. The use according to claim 9, characterized in that: The mechanical properties include one or more of tensile strength, tensile modulus, tensile yield strain, flexural strength, flexural modulus and flexural stiffness.
Citation Information
Patent Citations
Bimodally-distributed glass fiber reinforced polypropylene composite material and preparation method thereof
CN104910517A
Ultra-light high-sound-absorption GMT reinforced PU thermoplastic automotive trim composite board and preparation method thereof
CN109823012A
Automobile hemp fiber ceiling and manufacturing process thereof
CN110802887A
Fiber-reinforced light thermoplastic interface-free layered felt material for passenger car interior and exterior decoration, device and preparation method
CN113684606A
LWRT composite board for motor home interior decoration
CN220808790U
Cited By
Preparation method of LWRT composite board, LWRT composite board and application of LWRT composite board
CN119502514A
Preparation method of LWRT composite board, LWRT composite board and application thereof
CN119502514B
Fiber reinforced thermoplastic composite material automotive interior ceiling and preparation method thereof
CN119610818A
A fiber-reinforced thermoplastic composite automotive interior ceiling and its preparation method
CN119610818B