Composite pipe containing carbon fibers and production process thereof

By adopting the three-layer structure design of carbon fiber composite pipes in the pipeline, the problems of corrosion and weight of traditional metal pipes in high pressure, high temperature or special environments are solved, and high-performance lightweight pipes are realized, with excellent strength and durability sex.

CN118876508APending Publication Date: 2024-11-01ZHEJIANG AIYU NEW MATERIALS CO LTD

Patent Information

Application Number
CN202411071893.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Traditional metal pipes are prone to corrosion under high pressure, high temperature or special chemical environments and have a large weight, which cannot meet the needs of modern industry for high-performance pipes.

Method used

Using a composite tube containing carbon fiber, it is designed through a three-layer structure of the inner lining layer, reinforcement layer and outer protective layer. The inner lining layer is prepared by mixing polytetrafluoroethylene and polyimide, and the reinforcement layer is woven and wound by carbon fiber and glass fiber. , the outer protective layer is glass fiber reinforced plastic or polyethylene, and a tightly bonded composite tube is formed through winding molding and heating and pressurization processes.

Benefits of technology

It achieves the improvement of the strength, modulus and corrosion resistance of the pipe while maintaining light weight, extends the service life, and ensures that it meets design requirements and quality standards through quality inspection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118876508A_ABST
    Figure CN118876508A_ABST
Patent Text Reader

Abstract

The invention discloses a carbon fiber-containing composite pipe and a production process thereof, the carbon fiber-containing composite pipe comprises a lining layer, a reinforcing layer is arranged on the surface of the lining layer, an outer protective layer is arranged on the surface of the reinforcing layer, and the lining layer, the reinforcing layer and the outer protective layer are of an integrated structure. The lining layer is prepared by mixing polytetrafluoroethylene and polyimide, the reinforcing layer is prepared by mixing a carbon fiber bundle, a glass fiber bundle and a resin matrix, the reinforcing layer is formed by weaving the carbon fiber bundle and the glass fiber bundle into a reinforcing belt, then the reinforcing belt is wound on the surface of the lining layer, and the outer protective layer is made of glass fiber reinforced plastic or polyethylene. The invention relates to the technical field of composite materials. The composite pipe containing the carbon fibers has excellent strength and durability; according to the production technology of the composite pipe containing the carbon fibers, the technological means of winding forming, heating and pressurizing are adopted, tight combination of all the layers is achieved, and the overall performance of the composite pipe is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of composite materials, in particular to a composite tube containing carbon fibers and a production process thereof. Background Art

[0002] A pipeline is a device connected by pipes, pipe connectors and valves for conveying gas, liquid or fluid with solid particles. Pipes are widely used, mainly in water supply, drainage, heating, gas supply, long-distance transportation of oil and natural gas, agricultural irrigation, hydraulic engineering and various industrial devices. With the continuous progress of material science, carbon fiber, as a lightweight and high-strength material, has been widely used in aerospace, automobile, sports equipment and other fields. However, in the field of pipeline systems, especially pipelines that need to withstand high pressure, high temperature or special chemical environments, traditional metal pipelines have gradually failed to meet the high performance requirements of modern industry for pipeline materials due to their disadvantages such as heavy weight and easy corrosion. Therefore, the present invention aims to provide a composite pipe containing carbon fiber and a production process thereof to meet the demand for high-performance pipelines in the above-mentioned fields. Summary of the invention

[0003] 1. Technical issues to be solved

[0004] In view of the shortcomings of the prior art, the present invention provides a composite pipe containing carbon fiber and a production process thereof, aiming to solve the problems of heavy weight and easy corrosion of traditional metal pipes, while improving the strength, modulus and corrosion resistance of the pipe.

[0005] (II) Technical solution

[0006] To achieve the above objectives, the present invention is implemented through the following technical scheme: a composite tube containing carbon fiber, including an inner lining layer, a reinforcing layer is arranged on the surface of the inner lining layer, an outer protective layer is arranged on the surface of the reinforcing layer, the inner lining layer, the reinforcing layer and the outer protective layer are an integrated structure, and the surface of the outer protective layer is provided with raised ribs.

[0007] The inner lining layer is prepared by mixing polytetrafluoroethylene and polyimide, and the reinforcing layer is prepared by mixing carbon fiber bundles, glass fiber bundles and resin matrix. The reinforcing layer is first woven into a reinforcing belt by weaving carbon fiber bundles and glass fiber bundles, and then the reinforcing belt is wrapped around the surface of the inner lining layer. The outer protective layer adopts glass fiber reinforced plastic or polyethylene.

[0008] Preferably, the weight ratio of the polytetrafluoroethylene to the polyimide is 1:0.2 to 1:5.

[0009] Preferably, the weight ratio of the carbon fiber bundle to the glass fiber bundle is 1:0.2 to 1:1.

[0010] Preferably, the reinforcement tape is woven by a plain needle weaving method, and its warp and weft are a mixture of carbon fiber bundles and glass fiber bundles.

[0011] Preferably, the winding mode of the reinforcement tape is one of parallel winding, spiral winding, vertical winding and angle cross winding.

[0012] A production process for a composite tube containing carbon fibers comprises the following steps:

[0013] S1. Preparation of the inner lining layer: After pretreatment, polytetrafluoroethylene and polyimide are placed in a mixer for stirring, the mixed materials are placed in a pipe mold, and the mold is placed in a hot press, heated and pressurized, and demolded after cooling to produce the inner lining layer;

[0014] S2, preparation of reinforcement layer: pre-treating carbon fiber bundles and glass fiber bundles; blending the pre-treated carbon fiber bundles and glass fiber bundles according to a proportion, and then weaving them into reinforcement tapes, mixing the reinforcement tapes with the resin matrix evenly, placing the prepared lining layer in a winding device, using the winding device to wind the reinforcement tape on the lining layer according to a predetermined winding method, placing the wound composite pipe in a hot pressing device, and heating and pressurizing the wound layers to make them tightly bonded to each other and to the lining layer to form a reinforcement layer;

[0015] S3. Preparation of protective layer: glass fiber reinforced plastic or polyethylene is used to make a protective pipe, whose inner diameter is larger than the outer diameter of the reinforcement layer, epoxy resin is evenly applied on the surface of the reinforcement layer, the protective pipe is sheathed on the surface of the reinforcement layer, and a composite pipe is prepared after heating and curing;

[0016] S4, cutting and grinding: cutting the composite pipe according to the specific length and size requirements, and grinding the cut composite pipe to remove burrs and uneven parts on the surface;

[0017] S5. Quality inspection: Carry out quality inspection on the composite pipe, including size measurement, strength test, corrosion resistance test, etc., to ensure that it meets the design requirements and quality standards.

[0018] Preferably, in step S1, the pretreatment of polytetrafluoroethylene and polyimide includes drying, the drying temperature is 50-80°C, the drying time is 30-100 min, the heating temperature of the hot press is 360-400°C, and the holding pressure is 50-200 Kg / cm 2 , the holding time is 30-70min.

[0019] Preferably, in step S2, the pretreatment of the carbon fiber bundle and the glass fiber bundle includes cleaning, drying and surface activation, the winding method adopts one of parallel winding, spiral winding, vertical winding and angle cross winding, the number of winding layers is 2-8 layers, the heating temperature in the hot pressing equipment is 80-130°C, the heating time is 30-60min, and the pressure is 20-100Kg / cm 2 .

[0020] Preferably, the inner diameter of the protective pipe prepared in step S3 is 0.2-3 mm larger than the outer diameter of the reinforcement layer.

[0021] (III) Beneficial effects

[0022] The present invention provides a composite tube containing carbon fiber and a production process thereof. It has the following beneficial effects:

[0023] (1) This composite pipe containing carbon fiber forms a unique three-layer structure by arranging a reinforcement layer on the outside of the inner lining layer and an outer protective layer on the outside of the reinforcement layer, so that the composite pipe has excellent strength and durability while maintaining light weight; the inner lining layer is prepared by mixing polytetrafluoroethylene and polyimide, and has the characteristics of corrosion resistance and high temperature resistance; the reinforcement layer is woven into a reinforcement belt by carbon fiber bundles and glass fiber bundles, and the reinforcement belt is then impregnated with a resin matrix and wrapped around the surface of the inner lining layer, thereby improving the utilization rate of the carbon fiber and the strength and modulus of the composite pipe; the outer layer is made of corrosion-resistant and wear-resistant materials, which improves the corrosion resistance and service life of the composite pipe.

[0024] (2) The production process of the composite tube containing carbon fiber achieves close bonding between the layers by adopting winding molding and heating and pressurizing process means, thereby improving the overall performance of the composite tube. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is a schematic diagram of the structure of the composite tube of the present invention.

[0026] In the figure: 1- lining layer, 2- reinforcing layer, 3- outer protective layer. DETAILED DESCRIPTION

[0027] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] Embodiment 1:

[0029] A composite tube containing carbon fiber comprises an inner lining layer 1, a reinforcing layer 2 is arranged on the surface of the inner lining layer 1, an outer protective layer 3 is arranged on the surface of the reinforcing layer 2, and the inner lining layer 1, the reinforcing layer 2 and the outer protective layer 3 are an integrated structure;

[0030] The inner lining layer 1 is prepared by mixing polytetrafluoroethylene and polyimide, and the reinforcing layer 2 is prepared by mixing carbon fiber bundles, glass fiber bundles and resin matrix. The reinforcing layer 2 is first woven into a reinforcing belt by carbon fiber bundles and glass fiber bundles, and then the reinforcing belt is wrapped around the surface of the inner lining layer 1. The outer protective layer 3 adopts glass fiber reinforced plastic or polyethylene.

[0031] The weight ratio of polytetrafluoroethylene to polyimide is 1:0.2.

[0032] The weight ratio of carbon fiber bundles to glass fiber bundles is 1:0.2.

[0033] The reinforcement tape is woven using a flat needle weave method, and its warp and weft threads are made of a mixture of carbon fiber bundles and glass fiber bundles.

[0034] The winding mode of the reinforcement tape is one of parallel winding, spiral winding, vertical winding and angle cross winding.

[0035] A production process of a composite tube containing carbon fiber, characterized in that it comprises the following steps:

[0036] S1. Preparation of the inner lining layer: After pretreatment, polytetrafluoroethylene and polyimide are placed in a mixer for stirring, the mixed materials are placed in a pipe mold, and the mold is placed in a hot press, heated and pressurized, and demolded after cooling to produce the inner lining layer;

[0037] S2, preparation of reinforcement layer: pre-treating carbon fiber bundles and glass fiber bundles; blending the pre-treated carbon fiber bundles and glass fiber bundles according to a proportion, and then weaving them into reinforcement tapes, mixing the reinforcement tapes with the resin matrix evenly, placing the prepared lining layer in a winding device, using the winding device to wind the reinforcement tape on the lining layer according to a predetermined winding method, placing the wound composite pipe in a hot pressing device, and heating and pressurizing the wound layers to make them tightly bonded to each other and to the lining layer to form a reinforcement layer;

[0038] S3. Preparation of protective layer: glass fiber reinforced plastic or polyethylene is used to make a protective pipe, whose inner diameter is larger than the outer diameter of the reinforcement layer, epoxy resin is evenly applied on the surface of the reinforcement layer, the protective pipe is sheathed on the surface of the reinforcement layer, and a composite pipe is prepared after heating and curing;

[0039] S4, cutting and grinding: cutting the composite pipe according to the specific length and size requirements, and grinding the cut composite pipe to remove burrs and uneven parts on the surface;

[0040] S5. Quality inspection: Carry out quality inspection on the composite pipe, including size measurement, strength test, corrosion resistance test, etc., to ensure that it meets the design requirements and quality standards.

[0041] In step S1, the pretreatment of polytetrafluoroethylene and polyimide includes drying, the drying temperature is 50°C, the drying time is 30 minutes, the heating temperature of the hot press is 360°C, and the holding pressure is 50Kg / cm 2 , the holding time is 30min.

[0042] In step S2, the pretreatment of the carbon fiber bundle and the glass fiber bundle includes cleaning, drying and surface activation. Cleaning can remove impurities and oil stains on the surface, drying ensures that the resin can be fully absorbed in the subsequent resin infiltration process, and surface activation can enhance the interface bonding strength between the fiber and the resin matrix.

[0043] The winding method is one of parallel winding, spiral winding, vertical winding and angle cross winding. The number of winding layers is 2. The heating temperature in the hot pressing equipment is 80℃, the heating time is 30min, and the pressure is 20Kg / cm 2 .

[0044] The inner diameter of the protective pipe prepared in step S3 is 0.2 mm larger than the outer diameter of the reinforcing layer, which ensures that the protective pipe can be sleeved on the outside of the reinforcing layer.

[0045] Embodiment 2:

[0046] Different from the first embodiment, the weight ratio of polytetrafluoroethylene to polyimide is 1:2, and the weight ratio of carbon fiber bundle to glass fiber bundle is 1:0.5.

[0047] The drying temperature is 65℃, the drying time is 65min, the heating temperature of the hot press is 380℃, and the holding pressure is 120Kg / cm 2 , the holding time is 50min.

[0048] In step S2, the pretreatment of the carbon fiber bundle and the glass fiber bundle includes cleaning, drying and surface activation, the winding method adopts one of parallel winding, spiral winding, vertical winding and angle cross winding, the number of winding layers is 5, the heating temperature in the hot pressing equipment is 110°C, the heating time is 45min, and the pressure is 60Kg / cm 2 .

[0049] The inner diameter of the protective pipe prepared in step S3 is 1.5 mm larger than the outer diameter of the reinforcement layer.

[0050] Embodiment three:

[0051] Different from the first embodiment, the weight ratio of polytetrafluoroethylene to polyimide is 1:5, and the weight ratio of carbon fiber bundle to glass fiber bundle is 1:1.

[0052] The drying temperature is 80℃, the drying time is 100min, the heating temperature of the hot press is 400℃, and the holding pressure is 200Kg / cm 2 , the holding time is 70min.

[0053] In step S2, the pretreatment of the carbon fiber bundle and the glass fiber bundle includes cleaning, drying and surface activation. The winding method adopts one of parallel winding, spiral winding, vertical winding and angle cross winding. The number of winding layers is 8. The heating temperature in the hot pressing equipment is 130°C, the heating time is 60 minutes, and the pressure is 100Kg / cm 2 .

[0054] The inner diameter of the protective pipe prepared in step S3 is 0.2-3 mm larger than the outer diameter of the reinforcement layer.

[0055] Comparative Example 1:

[0056] Different from the first embodiment, the carbon fiber bundle and the glass fiber bundle are directly impregnated in the resin and wound around the surface of the inner lining layer.

[0057] Comparative Example 2:

[0058] The difference from the first embodiment is that glass fiber reinforced plastic is used as the reinforcement layer, and the thickness of the reinforcement layer is the same as that of the first embodiment.

[0059] Comparative Example 3:

[0060] Different from the first embodiment, only carbon fiber bundles are used as the raw material of the reinforcement layer.

[0061] The axial tensile strength and elastic modulus of the composite pipes of the embodiment and the comparative example were measured, and the measurement results were as follows:

[0062] Group Tensile strength(MPa) Elastic modulus(GPa) Embodiment 1 2955 265 Embodiment 2 3157 281 Embodiment 3 3305 294 Comparative Example 1 2650 238 Comparative Example 2 2597 226 Comparative Example 3 2628 232

[0063] It can be seen from the above table that the composite pipe of the embodiment of the present invention has excellent performance and has good tensile strength and impact strength.

[0064] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the statement "comprise a ..." do not exclude the presence of other identical elements in the process, method, article or device including the elements.

[0065] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A composite tube containing carbon fibers, characterized in that: The invention comprises an inner lining layer (1), a reinforcing layer (2) is arranged on the surface of the inner lining layer (1), an outer protective layer (3) is arranged on the surface of the reinforcing layer (2), and the inner lining layer (1), the reinforcing layer (2) and the outer protective layer (3) are an integrated structure; The inner lining layer (1) is prepared by mixing polytetrafluoroethylene and polyimide, and the reinforcing layer (2) is prepared by mixing carbon fiber bundles, glass fiber bundles and a resin matrix. The reinforcing layer (2) is first woven into a reinforcing belt by the carbon fiber bundles and the glass fiber bundles, and then the reinforcing belt is wound on the surface of the inner lining layer (1). The outer protective layer (3) is made of glass fiber reinforced plastic or polyethylene.

2. A composite tube containing carbon fibers according to claim 1, characterized in that: The weight ratio of the polytetrafluoroethylene to the polyimide is 1:0.2 to 1:

5.

3. The composite tube containing carbon fibers according to claim 1, characterized in that: The weight ratio of the carbon fiber bundle to the glass fiber bundle is 1:0.2 to 1:

1.

4. A composite tube containing carbon fibers according to claim 3, characterized in that: The reinforcement tape is woven using a flat needle weave method, and its warp and weft threads are made of a mixture of carbon fiber bundles and glass fiber bundles.

5. The composite tube containing carbon fibers according to claim 1, characterized in that: The winding mode of the reinforcement tape is one of parallel winding, spiral winding, vertical winding and angle cross winding.

6. A process for producing a composite tube containing carbon fibers according to any one of claims 1 to 5, characterized in that: The following steps are involved: S1. Preparation of the inner lining layer: After pretreatment, polytetrafluoroethylene and polyimide are placed in a mixer and stirred, the mixed materials are placed in a pipe mold, and the mold is placed in a hot press, heated and pressurized, and demolded after cooling to produce the inner lining layer; S2, preparation of reinforcement layer: pre-treating carbon fiber bundles and glass fiber bundles; blending the pre-treated carbon fiber bundles and glass fiber bundles according to a proportion, and then weaving them into reinforcement tapes, mixing the reinforcement tapes with the resin matrix evenly, placing the prepared lining layer in a winding device, using the winding device to wind the reinforcement tape on the lining layer according to a predetermined winding method, placing the wound composite pipe in a hot pressing device, and heating and pressurizing the wound layers to make them tightly bonded to each other and to the lining layer to form a reinforcement layer; S3. Preparation of protective layer: glass fiber reinforced plastic or polyethylene is used to make a protective pipe, whose inner diameter is larger than the outer diameter of the reinforcement layer, epoxy resin is evenly applied on the surface of the reinforcement layer, the protective pipe is sheathed on the surface of the reinforcement layer, and a composite pipe is prepared after heating and curing; S4, cutting and grinding: cutting the composite pipe according to the specific length and size requirements, and grinding the cut composite pipe to remove burrs and uneven parts on the surface; S5. Quality inspection: Carry out quality inspection on the composite pipe, including size measurement, strength test, corrosion resistance test, etc., to ensure that it meets the design requirements and quality standards.

7. The production process of a composite tube containing carbon fiber according to claim 6, characterized in that: In step S1, the pretreatment of polytetrafluoroethylene and polyimide includes drying, the drying temperature is 50-80°C, the drying time is 30-100 minutes, the heating temperature of the hot press is 360-400°C, and the holding pressure is 50-200Kg / cm 2 , the holding time is 30-70min.

8. The production process of a composite tube containing carbon fibers according to claim 6, characterized in that: In step S2, the pretreatment of the carbon fiber bundle and the glass fiber bundle includes cleaning, drying and surface activation, the winding method adopts one of parallel winding, spiral winding, vertical winding and angle cross winding, the number of winding layers is 2-8 layers, the heating temperature in the hot pressing equipment is 80-130°C, the heating time is 30-60min, and the pressure is 20-100Kg / cm 2 .

9. The process for producing a composite tube containing carbon fibers according to claim 6, characterized in that: The inner diameter of the protective pipe prepared in step S3 is 0.2-3 mm larger than the outer diameter of the reinforcement layer.

Citation Information

Patent Citations

  • Abrasion-resistant fluoroplastic sleeve

    CN101672395A

  • Continuous filament wound and reinforced thermoplastic pipe and manufacturing process thereof

    CN102679047A

  • Method for preparing tube blank of holder by polyimide with nano-copper and polytetrafluoroethylene

    CN103101205A

  • Fiber guide pipe with far-infrared heating function

    CN103527863A

  • Preparation method of tubular polyimide composite material for bearing retainers

    CN104046024A

Cited By

  • Preparation method of prestressed fiber reinforced wood-bamboo-based ship pressure pipeline

    CN121798949A