High-reflectivity ABS material and preparation method thereof

By introducing air with a low refractive index into the ABS resin and forming micro-holes by chemical etching, the mechanical performance degradation caused by inorganic fillers in traditional reflective materials is solved, and a combination of high reflectivity and excellent mechanical properties is achieved.

CN118876534APending Publication Date: 2024-11-01NANJING JULONG SCIENCE & TECHNOLOGY CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410965969.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The introduction of inorganic fillers in traditional reflective materials has led to a decline in mechanical properties, which cannot meet the needs of diversified use scenarios. In addition, nano-scale inorganic fillers are costly and have poor dispersion performance, making it difficult to achieve an ideal light reflection effect.

Method used

By introducing air with a lower refractive index into the ABS resin substrate, chemical etching is used to form uniformly distributed micro-holes to create a high reflective layer, and using the difference in refractive index between resin and air to achieve a high reflective effect, avoiding the mechanical use of inorganic fillers Negative effects of performance.

Benefits of technology

The light reflection effect of high reflectivity ABS material is achieved, while maintaining excellent mechanical properties, avoiding the material embrittlement problem caused by excessive addition of inorganic fillers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118876534A_ABST
    Figure CN118876534A_ABST
Patent Text Reader

Abstract

The invention relates to the field of reflective materials, and particularly discloses a high-reflectivity ABS material and a preparation method thereof. The high-reflectivity ABS material comprises an ABS base layer and an ABS high-reflection layer, wherein the ABS high-reflection layer is prepared from the following raw materials in percentage by mass: 86-90% of ABS resin, 8-12% of spherical calcium carbonate and 1-3% of auxiliaries; holes formed through chemical etching are distributed in the surface of the ABS high-reflection layer; the preparation method comprises the following steps: uniformly mixing the ABS resin, the spherical calcium carbonate and the auxiliary agent according to the ratio, and extruding to obtain the calcium carbonate / ABS composite resin; co-extruding the calcium carbonate / ABS composite resin and ABS resin to obtain a composite board; and carrying out chemical etching on the surface of the composite board by using an acid solution, and washing by using weakly alkaline water and pure water respectively to obtain the high-reflectivity ABS material. The high-reflectivity ABS material provided by the invention has the advantages of good reflectivity and excellent mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of reflective materials, and more specifically, to a high-reflectivity ABS material and a preparation method thereof. Background Art

[0002] Reflective materials are widely used in building panels and other fields. ABS resin has excellent appearance, mechanical properties, chemical resistance, dimensional stability and coloring properties, and commercialized ABS resins of different grades have adjustable flame retardant, high gloss, heat resistance, high impact, etc. Therefore, ABS resin is a good choice for the resin substrate of reflective materials.

[0003] Common reflective materials are made by adding reflective agents and other related additives to the resin substrate. The reflective agent is generally selected as rutile titanium dioxide and barium sulfate. By using reflective fillers with high refractive index, the disadvantage of insufficient reflectivity of the resin polymer substrate is improved to achieve the purpose of high reflectivity. However, inorganic filler reflective agents need to be added in a large amount to achieve a better reflective effect, but at the same time, they will greatly deteriorate the mechanical properties of the resin substrate, especially the impact resistance, causing the embrittlement of the reflective material and unable to meet the needs of more usage scenarios. In other cases, in related technologies, based on the principle of rigid toughening, nano-scale inorganic filler reflective agents are used to improve the brittleness of reflective materials. However, on the one hand, the cost of nano-scale inorganic materials is relatively high, and on the other hand, the dispersion performance of nano-scale inorganic fillers with a high addition amount is poor, and it is easy to agglomerate in the resin matrix, which will still cause the impact performance of the reflective material to decrease, and the ideal application effect cannot be achieved.

[0004] Regarding the above-mentioned related technologies, the inventors believe that the fundamental principle of the high refractive index of reflective materials lies in the difference in refractive indices between different raw materials. The high reflectivity of traditional reflective materials is actually caused by the difference between inorganic fillers with high refractive index and resin matrix with low refractive index. However, there are still many problems in the introduction of inorganic fillers. Therefore, the inventors creatively introduced air with a lower refractive index into the resin substrate evenly through etching, and used the difference in refractive index between resin and air to create a high reflective layer to achieve the purpose of reflection, while taking into account the mechanical properties of the material itself. Summary of the invention

[0005] In order to provide a high-reflectivity ABS material with better mechanical properties, the present application provides a high-reflectivity ABS material and a preparation method thereof.

[0006] In the first aspect, the present application provides a high reflectivity ABS material, which adopts the following technical solution:

[0007] A high-reflectivity ABS material, comprising an ABS base layer and an ABS high-reflection layer, wherein the ABS high-reflection layer comprises the following raw materials in percentage by mass: 86-90% ABS resin, 8-12% spherical calcium carbonate, and 1-3% additive;

[0008] The surface of the ABS high-reflection layer is distributed with holes formed by chemical etching.

[0009] Preferably, the cavities are micron cavities, and the cavities are evenly dispersed on the surface of the ABS high-reflection layer.

[0010] By adopting the above technical solution, the refractive index of air is about 1.0, and the refractive index of ABS resin is 1.6. The voids generated after etching have a large refractive index difference with the ABS resin. The voids are evenly distributed on the surface of the ABS high-reflective layer by etching, so that the ABS high-reflective layer has excellent light reflection effect, thereby avoiding the degradation effect of inorganic filler reflective agents on the mechanical properties of ABS materials.

[0011] Preferably, the particle size of the spherical calcium carbonate is 3000-5000 mesh.

[0012] Preferably, the particle size of the spherical calcium carbonate is 4000 mesh.

[0013] By adopting the above technical scheme, the particle size of spherical calcium carbonate in the range of 3000-5000 mesh can be dispersed relatively evenly in the ABS resin matrix, and can ensure that the surface of the ABS high reflective layer after etching has a suitable distribution of voids; when the particle size of the spherical calcium carbonate is too large, the number of particles of the spherical calcium carbonate under the same mass is small, and it is difficult to ensure that the spherical calcium carbonate can be distributed on the surface of the plate in the form of microspheres, and further it is difficult to ensure that the surface of the ABS high reflective layer after etching has a sufficient distribution of voids; when the particle size of the spherical calcium carbonate is too small, the dispersion uniformity of the spherical calcium carbonate decreases, and it is easy to agglomerate, which affects the mechanical properties of the plate and reduces the etching effect; the inventors found through experiments that when the particle size of the spherical calcium carbonate is 4000 mesh, the ABS material has the best light reflection effect and good mechanical properties.

[0014] Preferably, the chemical etching is performed using an acid solution, and the acid solution is selected from one of a sulfuric acid solution, a hydrochloric acid solution, and a nitric acid solution.

[0015] Preferably, the acid solution used in the acid etching is a sulfuric acid solution, and the concentration of the sulfuric acid solution is 2-5 mol / L.

[0016] By adopting the above technical scheme, the acid solution reacts with the spherical calcium carbonate on the surface of the ABS high reflective layer, the calcium carbonate is dissolved, and cavities are formed on the surface of the ABS high reflective layer; the reaction of the sulfuric acid solution with the spherical calcium carbonate is more stable, which is conducive to ensuring the etching quality; by controlling the concentration of the sulfuric acid solution, the etching reaction is made more stable, and the etching quality is further improved.

[0017] Preferably, the melt flow rate of the ABS resin is 4-6 (220°C, 10kg) g / 10min, and the impact strength is above 30KJ / m2.

[0018] Preferably, the auxiliary agents include anti-light aging agents, antioxidants, and lubricants.

[0019] Preferably, based on the total mass of the raw materials of the ABS high-reflection layer, the auxiliary agent includes 0.8-1.4% of an anti-light aging agent, 0.1-0.8% of an antioxidant, and 0.1-0.8% of a lubricant.

[0020] Preferably, the anti-light aging agent is a mixture of hindered amine light stabilizer 770 and ultraviolet absorber UV234 in a mass ratio of 1:1.

[0021] Preferably, the antioxidant is a mixture of antioxidant 1076 and antioxidant 168 in a mass ratio of 1:1.

[0022] Preferably, the lubricant is selected from one or more of EBS, PETS and silicone masterbatch.

[0023] Preferably, the thickness ratio of the ABS high reflective layer to the ABS base layer is (1:9)-(2:8). Further preferably, the thickness ratio of the ABS high reflective layer to the ABS base layer can be (1:9), (1.2:8.8), (1.25:8.75), (1.5:8.5), (1.75:8.25), or (2:8), which can be adjusted and selected according to actual application needs.

[0024] In a second aspect, the present application provides a method for preparing a high reflectivity ABS material, using the following technical solution:

[0025] A method for preparing a high-reflectivity ABS material comprises the following steps:

[0026] According to the proportion, ABS resin, spherical calcium carbonate and additives are mixed evenly and extruded to obtain calcium carbonate / ABS composite resin;

[0027] The calcium carbonate / ABS composite resin and the ABS resin are respectively put into a multi-layer co-extrusion extruder for co-extrusion to obtain a calcium carbonate / ABS layer-ABS base composite sheet;

[0028] At 40-60°C, the surface of the composite plate is chemically etched with an acid solution, and then washed with weak alkaline water and pure water respectively to obtain a high-reflectivity ABS material.

[0029] By adopting the above technical scheme, the surface of the calcium carbonate / ABS layer-ABS base composite board is chemically etched with an acid solution, and the spherical calcium carbonate on the surface of the calcium carbonate / ABS layer reacts with the acid solution and dissolves to generate in-situ voids, so that the surface of the calcium carbonate / ABS layer is evenly and abundantly distributed with micron voids, forming an ABS high-reflection layer with excellent light reflection effect.

[0030] Preferably, the mass ratio of the calcium carbonate / ABS composite resin to the ABS resin is (1:9)-(2:8).

[0031] Preferably, the processing time of the chemical etching step is 8-15 minutes.

[0032] Preferably, the weak alkaline water is selected from ammonia water and sodium bicarbonate solution, and the pH value of the weak alkaline water is 7.5-9.

[0033] In summary, this application has the following beneficial effects:

[0034] 1. The present application uses etching to utilize the reaction between an acid solution and spherical calcium carbonate, so that the in-situ voids formed after the dissolution of the spherical calcium carbonate are evenly distributed on the surface of the ABS high-reflection layer, and utilizes the difference in refractive index between air and the ABS resin matrix to make the ABS high-reflection layer have excellent light reflection effect. While ensuring that the ABS material has excellent surface light reflection performance, the possibility of a decrease in the mechanical properties of the ABS material caused by excessive addition of an inorganic filler reflective agent is avoided;

[0035] 2. The present application controls the particle size and addition amount of spherical calcium carbonate so that the spherical calcium carbonate can be evenly dispersed on the surface of the ABS high-reflection layer, and after etching, evenly dispersed voids are formed, so that the ABS high-reflection layer has excellent surface light reflection effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 This is a surface microscope inspection picture of the high reflectivity ABS material of Example 1 of the present application. DETAILED DESCRIPTION

[0037] To further help understand the technical solution of the present invention, the technical solution of the present invention is described in more detail below by providing several specific implementation examples. All of these described embodiments are only partial embodiments of the present invention, not all of them.

[0038] The following specific embodiments may be combined with each other, and the same or similar concepts or processes may not be described in detail in some embodiments; and the reaction devices, monomer compounds, etc. involved in the following embodiments are all commercially available.

[0039] The following specific embodiments may be combined with each other, and the same or similar concepts or processes therein may not be described in detail in some embodiments.

[0040] The following examples are further explanations of the present invention, but the present invention is not limited thereto. Unless otherwise specified in the examples, the percentages are all by mass.

[0041] Example

[0042] Example 1

[0043] This embodiment discloses a high reflectivity ABS material, and the preparation method is as follows:

[0044] 88 parts by mass of ABS resin, 10 parts by mass of 4000 mesh spherical calcium carbonate, 1 part by mass of anti-light aging agent, 0.5 parts by mass of antioxidant, and 0.5 parts by mass of lubricant are put into a high-speed mixer, mixed evenly, and then extruded and granulated by a twin-screw extruder to obtain a calcium carbonate / ABS composite resin; in this embodiment, the model of the ABS resin is Trinseo A460, the anti-light aging agent is a mixture of hindered amine light stabilizer 770 and ultraviolet absorber UV234 in a mass ratio of 1:1, the antioxidant is a mixture of antioxidant 1076 and antioxidant 168 in a mass ratio of 1:1, and the lubricant is a silicone masterbatch;

[0045] Calcium carbonate / ABS composite resin and ABS resin are put into a multi-layer extruder at a mass ratio of 1:9, and co-extruded to obtain a calcium carbonate / ABS layer-ABS layer composite sheet; in this embodiment, the ABS resin is Trinseo A460;

[0046] At 50°C, the calcium carbonate / ABS layer-ABS layer composite board was immersed in a 4 mol / L sulfuric acid solution and etched for 10 minutes. The etched board was then taken out and washed three times with a sodium bicarbonate solution with a pH value of 8 and pure water respectively to obtain a high-reflectivity ABS material with an ABS high-reflection layer-ABS base composite structure.

[0047] Reference Figure 1 It can be seen that there are abundant micron voids distributed on the high reflective surface of the ABS material with high reflectivity.

[0048] Example 2

[0049] The only difference between this embodiment and embodiment 1 is that the preparation method of the high reflectivity ABS material is as follows:

[0050] 86 parts by weight of ABS resin, 12 parts by weight of 4000 mesh spherical calcium carbonate, 1 part by weight of light aging inhibitor, 0.5 parts by weight of antioxidant, and 0.5 parts by weight of lubricant are put into a high-speed mixer, mixed evenly, and then extruded and granulated by a twin-screw extruder to obtain a calcium carbonate / ABS composite resin;

[0051] The calcium carbonate / ABS composite resin and the ABS resin are put into a multi-layer extruder at a mass ratio of 1:9, and co-extruded to obtain a calcium carbonate / ABS layer-ABS layer composite sheet;

[0052] At 50°C, the calcium carbonate / ABS layer-ABS layer composite board was immersed in a 4 mol / L sulfuric acid solution and etched for 10 minutes. The etched board was then taken out and washed three times with a sodium bicarbonate solution with a pH value of 8 and pure water respectively to obtain a high reflectivity ABS material.

[0053] Example 3

[0054] The only difference between this embodiment and embodiment 1 is that the preparation method of the high reflectivity ABS material is as follows:

[0055] 90 parts by weight of ABS resin, 8 parts by weight of 4000 mesh spherical calcium carbonate, 1 part by weight of light aging agent, 0.5 parts by weight of antioxidant, and 0.5 parts by weight of lubricant are put into a high-speed mixer, mixed evenly, and then extruded and granulated by a twin-screw extruder to obtain a calcium carbonate / ABS composite resin;

[0056] The calcium carbonate / ABS composite resin and the ABS resin are put into a multi-layer extruder at a mass ratio of 1:9, and co-extruded to obtain a calcium carbonate / ABS layer-ABS layer composite sheet;

[0057] At 50°C, the calcium carbonate / ABS layer-ABS layer composite board was immersed in a 4 mol / L sulfuric acid solution and etched for 10 minutes. The etched board was then taken out and washed three times with a sodium bicarbonate solution with a pH value of 8 and pure water respectively to obtain a high reflectivity ABS material.

[0058] Example 4

[0059] The only difference between this embodiment and embodiment 1 is that the preparation method of the high reflectivity ABS material is as follows:

[0060] 88 parts by weight of ABS resin, 10 parts by weight of 3000 mesh spherical calcium carbonate, 1 part by weight of light aging inhibitor, 0.5 parts by weight of antioxidant, and 0.5 parts by weight of lubricant are put into a high-speed mixer, mixed evenly, and then extruded and granulated by a twin-screw extruder to obtain a calcium carbonate / ABS composite resin;

[0061] The calcium carbonate / ABS composite resin and the ABS resin are put into a multi-layer extruder at a mass ratio of 1:9, and co-extruded to obtain a calcium carbonate / ABS layer-ABS layer composite sheet;

[0062] At 50°C, the calcium carbonate / ABS layer-ABS layer composite board was immersed in a 4 mol / L sulfuric acid solution and etched for 10 minutes. The etched board was then taken out and washed three times with a sodium bicarbonate solution with a pH value of 8 and pure water respectively to obtain a high reflectivity ABS material.

[0063] Example 5

[0064] The only difference between this embodiment and embodiment 1 is that the preparation method of the high reflectivity ABS material is as follows:

[0065] 88 parts by weight of ABS resin, 10 parts by weight of 5000 mesh spherical calcium carbonate, 1 part by weight of light aging inhibitor, 0.5 parts by weight of antioxidant, and 0.5 parts by weight of lubricant are put into a high-speed mixer, mixed evenly, and then extruded and granulated by a twin-screw extruder to obtain a calcium carbonate / ABS composite resin;

[0066] The calcium carbonate / ABS composite resin and the ABS resin are put into a multi-layer extruder at a mass ratio of 1:9, and co-extruded to obtain a calcium carbonate / ABS layer-ABS layer composite sheet;

[0067] At 50°C, the calcium carbonate / ABS layer-ABS layer composite board was immersed in a 4 mol / L sulfuric acid solution and etched for 10 minutes. The etched board was then taken out and washed three times with a sodium bicarbonate solution with a pH value of 8 and pure water respectively to obtain a high reflectivity ABS material.

[0068] Example 6

[0069] The only difference between this embodiment and embodiment 1 is that the preparation method of the high reflectivity ABS material is as follows:

[0070] 88 parts by weight of ABS resin, 10 parts by weight of 5000 mesh spherical calcium carbonate, 1 part by weight of light aging inhibitor, 0.5 parts by weight of antioxidant, and 0.5 parts by weight of lubricant are put into a high-speed mixer, mixed evenly, and then extruded and granulated by a twin-screw extruder to obtain a calcium carbonate / ABS composite resin;

[0071] The calcium carbonate / ABS composite resin and the ABS resin are put into a multi-layer extruder at a mass ratio of 1:9, and co-extruded to obtain a calcium carbonate / ABS layer-ABS layer composite sheet;

[0072] At 50°C, the calcium carbonate / ABS layer-ABS layer composite board was immersed in a 4 mol / L hydrochloric acid solution and etched for 10 minutes. The etched board was then taken out and washed three times with a sodium bicarbonate solution with a pH value of 8 and pure water respectively to obtain a high reflectivity ABS material.

[0073] Example 7

[0074] The only difference between this embodiment and embodiment 1 is that the preparation method of the high reflectivity ABS material is as follows:

[0075] 88 parts by weight of ABS resin, 10 parts by weight of 5000 mesh spherical calcium carbonate, 1 part by weight of light aging inhibitor, 0.5 parts by weight of antioxidant, and 0.5 parts by weight of lubricant are put into a high-speed mixer, mixed evenly, and then extruded and granulated by a twin-screw extruder to obtain a calcium carbonate / ABS composite resin;

[0076] The calcium carbonate / ABS composite resin and the ABS resin are put into a multi-layer extruder at a mass ratio of 1:9, and co-extruded to obtain a calcium carbonate / ABS layer-ABS layer composite sheet;

[0077] At 50°C, the calcium carbonate / ABS layer-ABS layer composite board was immersed in a 4 mol / L nitric acid solution and etched for 10 minutes. The etched board was then taken out and washed three times with a sodium bicarbonate solution with a pH value of 8 and pure water respectively to obtain a high reflectivity ABS material.

[0078] Example 8

[0079] The only difference between this embodiment and embodiment 1 is that the preparation method of the high reflectivity ABS material is as follows:

[0080] 88 parts by weight of ABS resin, 10 parts by weight of 5000 mesh spherical calcium carbonate, 1 part by weight of light aging inhibitor, 0.5 parts by weight of antioxidant, and 0.5 parts by weight of lubricant are put into a high-speed mixer, mixed evenly, and then extruded and granulated by a twin-screw extruder to obtain a calcium carbonate / ABS composite resin;

[0081] The calcium carbonate / ABS composite resin and the ABS resin are put into a multi-layer extruder at a mass ratio of 1:9, and co-extruded to obtain a calcium carbonate / ABS layer-ABS layer composite sheet;

[0082] At 40°C, the calcium carbonate / ABS layer-ABS layer composite board was immersed in a 5 mol / L sulfuric acid solution and etched for 10 minutes. The etched board was then taken out and washed three times with a sodium bicarbonate solution with a pH value of 8 and pure water respectively to obtain a high reflectivity ABS material.

[0083] Example 9

[0084] The only difference between this embodiment and embodiment 1 is that the preparation method of the high reflectivity ABS material is as follows:

[0085] 88 parts by weight of ABS resin, 10 parts by weight of 5000 mesh spherical calcium carbonate, 1 part by weight of light aging inhibitor, 0.5 parts by weight of antioxidant, and 0.5 parts by weight of lubricant are put into a high-speed mixer, mixed evenly, and then extruded and granulated by a twin-screw extruder to obtain a calcium carbonate / ABS composite resin;

[0086] The calcium carbonate / ABS composite resin and the ABS resin are put into a multi-layer extruder at a mass ratio of 1:9, and co-extruded to obtain a calcium carbonate / ABS layer-ABS layer composite sheet;

[0087] At 60°C, the calcium carbonate / ABS layer-ABS layer composite board was immersed in a 3 mol / L sulfuric acid solution and etched for 10 minutes. The etched board was then taken out and washed three times with a sodium bicarbonate solution with a pH value of 8 and pure water respectively to obtain a high reflectivity ABS material.

[0088] Comparative Example

[0089] Comparative Example 1

[0090] A commercially available ABS-based reflective sheeting.

[0091] Comparative Example 2

[0092] The difference between this comparative example and comparative example 1 is that the preparation method of the high reflectivity ABS material is as follows:

[0093] 93 parts by weight of ABS resin, 5 parts by weight of 4000 mesh spherical calcium carbonate, 1 part by weight of light aging agent, 0.5 parts by weight of antioxidant, and 0.5 parts by weight of lubricant are put into a high-speed mixer, mixed evenly, and then extruded and granulated by a twin-screw extruder to obtain a calcium carbonate / ABS composite resin;

[0094] The calcium carbonate / ABS composite resin and the ABS resin are put into a multi-layer extruder at a mass ratio of 1:9, and co-extruded to obtain a calcium carbonate / ABS layer-ABS layer composite sheet;

[0095] At 50°C, the calcium carbonate / ABS layer-ABS layer composite board was immersed in a 4 mol / L sulfuric acid solution and etched for 10 minutes. The etched board was then taken out and washed three times with a sodium bicarbonate solution with a pH value of 8 and pure water respectively to obtain a high reflectivity ABS material.

[0096] Comparative Example 3

[0097] The difference between this comparative example and comparative example 1 is that the preparation method of the high reflectivity ABS material is as follows:

[0098] 83 parts by weight of ABS resin, 15 parts by weight of 4000 mesh spherical calcium carbonate, 1 part by weight of light aging inhibitor, 0.5 parts by weight of antioxidant, and 0.5 parts by weight of lubricant were put into a high-speed mixer, mixed evenly, and then extruded and granulated by a twin-screw extruder to obtain a calcium carbonate / ABS composite resin;

[0099] The calcium carbonate / ABS composite resin and the ABS resin are put into a multi-layer extruder at a mass ratio of 1:9, and co-extruded to obtain a calcium carbonate / ABS layer-ABS layer composite sheet;

[0100] At 50°C, the calcium carbonate / ABS layer-ABS layer composite board was immersed in a 4 mol / L sulfuric acid solution and etched for 10 minutes. The etched board was then taken out and washed three times with a sodium bicarbonate solution with a pH value of 8 and pure water respectively to obtain a high reflectivity ABS material.

[0101] Comparative Example 4

[0102] The difference between this comparative example and comparative example 1 is that the preparation method of the high reflectivity ABS material is as follows:

[0103] 88 parts by weight of ABS resin, 10 parts by weight of 2000 mesh spherical calcium carbonate, 1 part by weight of light aging inhibitor, 0.5 parts by weight of antioxidant, and 0.5 parts by weight of lubricant are put into a high-speed mixer, mixed evenly, and then extruded and granulated by a twin-screw extruder to obtain a calcium carbonate / ABS composite resin;

[0104] The calcium carbonate / ABS composite resin and the ABS resin are put into a multi-layer extruder at a mass ratio of 1:9, and co-extruded to obtain a calcium carbonate / ABS layer-ABS layer composite sheet;

[0105] At 50°C, the calcium carbonate / ABS layer-ABS layer composite board was immersed in a 4 mol / L sulfuric acid solution and etched for 10 minutes. The etched board was then taken out and washed three times with a sodium bicarbonate solution with a pH value of 8 and pure water respectively to obtain a high reflectivity ABS material.

[0106] Comparative Example 5

[0107] The difference between this comparative example and comparative example 1 is that the preparation method of the high reflectivity ABS material is as follows:

[0108] 88 parts by weight of ABS resin, 10 parts by weight of 8000 mesh spherical calcium carbonate, 1 part by weight of light aging inhibitor, 0.5 parts by weight of antioxidant, and 0.5 parts by weight of lubricant are put into a high-speed mixer, mixed evenly, and then extruded and granulated by a twin-screw extruder to obtain a calcium carbonate / ABS composite resin;

[0109] The calcium carbonate / ABS composite resin and the ABS resin are put into a multi-layer extruder at a mass ratio of 1:9, and co-extruded to obtain a calcium carbonate / ABS layer-ABS layer composite sheet;

[0110] At 50°C, the calcium carbonate / ABS layer-ABS layer composite board was immersed in a 4 mol / L sulfuric acid solution and etched for 10 minutes. The etched board was then taken out and washed three times with a sodium bicarbonate solution with a pH value of 8 and pure water respectively to obtain a high reflectivity ABS material.

[0111] Performance testing

[0112] Take the ABS materials in Examples 1-9 and Comparative Examples 1-5, cut the specimens, and test the density, melt index, tensile strength, impact strength, flexural strength, flexural modulus and reflectivity. The density test standard is ISO 1183, the melt index test standard is ISO 1133, the tensile strength test standard is IS0527, the impact strength test standard is ISO 180, the flexural strength and flexural modulus test standard is ISO 178, and the reflectivity test standard is ASTM D1003. The test results are summarized in Table 1.

[0113] Table 1

[0114]

[0115]

[0116] Combining Examples 1-9 and Comparative Example 1 and Table 1, it can be seen that the reflectivity of the ABS material disclosed in the present application is similar to that of the existing ABS reflective material, while the impact strength and tensile strength are more excellent and the mechanical properties are better.

[0117] It can be seen from Examples 1-3, Comparative Examples 2-3 and Table 1 that the addition amount of spherical calcium carbonate is controlled with reference to the formula disclosed in the present application, so that the ABS material can have better reflectivity and higher mechanical properties. When the amount of spherical calcium carbonate added is too little, the reflectivity of the ABS material is poor, which may be due to the fact that the spherical calcium carbonate is less distributed on the surface of the ABS high reflective layer, and the micron voids formed after etching are less, resulting in a decrease in the reflectivity of the ABS; when the amount of spherical calcium carbonate added is too much, the impact strength of the ABS material is poor, which may be due to the fact that too much spherical calcium carbonate is easy to agglomerate in the ABS resin matrix, affecting the mechanical properties of the ABS material.

[0118] It can be seen from Example 1, Examples 3-5, Comparative Examples 4-5 and Table 1 that by controlling the particle size of spherical calcium carbonate, the ABS material can have better light reflection performance and better mechanical strength. When the particle size of the spherical calcium carbonate is too small, the light reflectivity of the ABS material decreases; when the particle size of the spherical calcium carbonate is too large, the light reflectivity of the ABS material decreases, and the mechanical properties such as impact strength are poor.

[0119] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A high reflectivity ABS material, It is characterized in that It includes an ABS base layer and an ABS high-reflection layer, wherein the ABS high-reflection layer includes the following raw materials in percentage by mass: 86-90% of ABS resin, 8-12% of spherical calcium carbonate, and 1-3% of an additive; The surface of the ABS high-reflection layer is distributed with holes formed by chemical etching.

2. The high reflectivity ABS material according to claim 1, It is characterized in that The particle size of the spherical calcium carbonate is 3000-5000 meshes.

3. The high reflectivity ABS material according to claim 2, It is characterized in that The particle size of the spherical calcium carbonate is 4000 meshes.

4. The high reflectivity ABS material according to claim 1, It is characterized in that The chemical etching is performed by using an acid solution, and the acid solution is selected from one of sulfuric acid, hydrochloric acid and nitric acid.

5. The high reflectivity ABS material according to claim 4, It is characterized in that The acid used for the acid etching is sulfuric acid, and the concentration of the sulfuric acid is 2-5 mol / L.

6. The high reflectivity ABS material according to claim 4, It is characterized in that The cavities are micron cavities, and the cavities are evenly dispersed on the surface of the ABS high-reflection layer.

7. The high reflectivity ABS material according to claim 1, It is characterized in that The melt flow rate of the ABS resin is 4-6 (220°C, 10kg) g / 10min, and the impact strength is 30KJ / m 2 above.

8. The high reflectivity ABS material according to claim 1, It is characterized in that The auxiliary agents include anti-light aging agents, antioxidants and lubricants.

9. The high reflectivity ABS material according to claim 1, It is characterized in that The thickness ratio of the ABS high-reflection layer to the ABS base layer is (1:9)-(2:8).

10. A method for preparing the high reflectivity ABS material according to any one of claims 1 to 9, It is characterized in that The following steps are involved: According to the proportion, ABS resin, spherical calcium carbonate and additives are mixed evenly and extruded to obtain calcium carbonate / ABS composite resin; The calcium carbonate / ABS composite resin and the ABS resin are respectively put into a multi-layer co-extrusion extruder for co-extrusion to obtain a calcium carbonate / ABS layer-ABS base composite sheet; At 40-60°C, the surface of the composite plate is chemically etched with an acid solution, and then washed with weak alkaline water and pure water respectively to obtain a high-reflectivity ABS material.

Citation Information

Patent Citations

  • Back plate of improved backlight unit

    CN103162238A

  • Non-pigment-method porous high-reflection heat-insulation cooling PVC film and preparation method thereof

    CN111234296A

  • Efficient radiation cooling film with excellent weather resistance and preparation method thereof

    CN118306081A

  • Filler for light reflection porous film and light reflection porous film incorporated with the filler

    JP2006265472A

  • Reflecting adhesive tape

    JP2007145941A