Easily-torn composite packaging material for dairy products
By modifying the Schiff alkali coupling agent and crosslinker on nano zinc oxide, combined with high-speed solvent-free composite technology, dairy packaging materials with antibacterial and tear-free properties are prepared, which solves the problem of the susceptibility of microbial contamination and packaging of dairy products. The problem of difficulty in tearing the bag of the material can achieve efficient antibacterial and safe use in dairy packaging.
Patent Information
- Application Number
- CN202410919312.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-07-10
AI Technical Summary
Dairy products are susceptible to microbial contamination during storage and transportation. The traditional plastic film bag mouth is difficult to tear and the tear mouth is irregular, resulting in the leakage of packaging contents, limiting its application in the field of dairy packaging.
The nano zinc oxide is modified by using Schiff alkali coupling agent and crosslinking agent to enhance its interface compatibility with polyethylene and impart antibacterial properties. The composite with antibacterial and tear-free properties is prepared through high-speed solvent-free composite technology. membrane.
The prepared dairy products easy-to-tear composite packaging materials have excellent antibacterial properties and easy-to-tear properties, which can effectively inhibit the growth of E. coli and Staphylococcus aureus, and meet the oxygen permeability and hygiene standards of dairy packaging, and have practical application value. .
Smart Images

Figure CN118876542A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of research and development of dairy product packaging materials, and in particular to an easy-to-tear composite packaging material for dairy products. Background Art
[0002] Dairy products are rich in nutrients such as protein, milk fat, sugar, vitamins, etc., which are very easy to cause microbial contamination during storage and transportation. Therefore, it is urgent to find natural, effective and safe methods to inhibit the growth of harmful microorganisms.
[0003] Adding antimicrobial agents is the main means to improve the antimicrobial properties of food packaging materials. For example, the patent with publication number CN116082732A discloses an antimicrobial polyethylene food-grade packaging film and its preparation method. By introducing a composite antimicrobial agent (composed of modified nano-zirconium phosphate-loaded silver antimicrobial agent and nano-zinc oxide antimicrobial agent) into the polyethylene material, the overall antimicrobial ability of the plastic packaging bag can be effectively improved.
[0004] The search found that nano zinc oxide is an inorganic antibacterial material with safety, long-lasting effect and heat resistance, and is widely used in food and drug packaging. Schiff base has antibacterial, bactericidal, anti-tumor and antiviral biological activities and is often used as an organic antibacterial agent. Coumarin is a natural antioxidant widely found in plants and has excellent antioxidant activity.
[0005] In addition, traditional plastic films have defects such as difficult to open the bag mouth, difficult to tear with bare hands, irregular or jagged tearing after tearing, which may cause leakage of package contents, etc., which limits its practical use in the field of dairy product packaging. Biaxially oriented films such as biaxially oriented nylon film (BOPA), biaxially oriented polyester film (BOPET), biaxially oriented polypropylene film (BOPP), and biaxially oriented polyethylene film (BOPE) have excellent tearing properties, can be torn in two directions in both directions, and have neat tearing. They can be made into composite materials by dry compounding or solvent-free compounding with traditional plastic films, which can meet the requirements of easy tearing of packaging products. Summary of the invention
[0006] The present invention provides an easy-to-tear composite packaging material for dairy products. Nano zinc oxide is synthesized and modified by using a Schiff base coupling agent and a Schiff base cross-linking agent. On the one hand, the interfacial compatibility between the nano zinc oxide and a polyethylene matrix is enhanced, and on the other hand, the polyethylene is synergistically endowed with antibacterial properties. Subsequently, a high-speed solvent-free composite process is adopted to prepare a dairy product packaging material with antibacterial properties.
[0007] A method for preparing an easy-to-tear composite packaging material for dairy products comprises the following steps:
[0008] Step 1, preparing a composite antibacterial agent, wherein the preparation method comprises: synthesizing a Schiff base coupling agent, and using the Schiff base coupling agent to perform surface modification on hydroxylated nano zinc oxide particles;
[0009] Step 2: Using low-density polyethylene resin and composite antibacterial agent as raw materials, blending, melting, and extruding through a twin-screw extruder, and performing longitudinal and then transverse stretching treatment, and hot pressing and shaping to obtain a BOPE surface layer;
[0010] Using ethylene-vinyl alcohol copolymer resin and low-density polyethylene resin as raw materials, they are blended, melted, extruded and pelletized through a twin-screw extruder, and then cast into a film to obtain a barrier intermediate layer;
[0011] Low-density polyethylene resin and composite antibacterial agent are used as raw materials, blended, melted, extruded and pelletized through a twin-screw extruder, and then cast into a film to obtain a PE inner layer;
[0012] Step three, using a high-speed solvent-free composite process to bond the BOPE surface layer, the barrier middle layer and the PE inner layer to obtain a composite film, which is an easy-to-tear composite packaging material for dairy products.
[0013] Preferably, the preparation method of the composite antibacterial agent is: synthesizing a Schiff base coupling agent and a Schiff base cross-linking agent, and using the Schiff base coupling agent and the Schiff base cross-linking agent to jointly perform surface modification on hydroxylated nano zinc oxide particles to obtain the composite antibacterial agent.
[0014] Preferably, the preparation method of the Schiff base coupling agent is:
[0015] Step S3-1: using 7-hydroxycoumarin as a nucleophilic reagent, a bromine functional group of 2-bromoacetaldehyde reacts with a hydroxyl functional group of 7-hydroxycoumarin to generate a coumarin aldehyde monomer;
[0016] Step S3-2: using the Schiff base reaction mechanism, the amino functional group of 3-aminopropyltrimethoxysilane and the carbonyl functional group of the coumarin aldehyde monomer undergo a condensation reaction to generate a Schiff base coupling agent.
[0017] Preferably, the preparation method of the Schiff base cross-linking agent is:
[0018] Step S4-1: using 5,7-dihydroxycoumarin as a nucleophilic reagent, a bromine functional group of 2-bromoacetaldehyde and a hydroxyl functional group of 5,7-dihydroxycoumarin undergo a nucleophilic substitution reaction to generate a coumarin dialdehyde monomer;
[0019] Step S4-2: using the Schiff base reaction mechanism, the amino functional group of 3-aminopropyltrimethoxysilane and the carbonyl functional group of the coumarin dialdehyde monomer undergo a condensation reaction to generate a Schiff base crosslinking agent.
[0020] Preferably, the preparation process parameters of the composite film in step three are set as follows: composite speed of 300-500 m / min, composite temperature of 40-50° C., cooling temperature of 20-30° C., composite pressure of 0.3-0.5 MPa, and gluing pressure of 0.4-0.6 MPa.
[0021] The thickness of the easily tearable composite packaging material for dairy products prepared according to the method is 80 to 200 μm.
[0022] Preferably, the average tearing force of the easy-to-tear composite packaging material for dairy products is 0.9-1.2N.
[0023] Preferably, the easily tearable composite packaging material for dairy products has an antibacterial effect, and the bacteria are Escherichia coli or Staphylococcus aureus.
[0024] Beneficial Effects
[0025] The present invention first synthesizes a Schiff base coupling agent and a cross-linking agent, uses the coupling agent and the cross-linking agent to perform surface modification on nano zinc oxide particles to obtain a composite antibacterial agent, then performs modification treatment on the surface layer and the inner layer of the composite film by the composite antibacterial agent, and finally adopts a high-speed solvent-free composite process to prepare the composite film;
[0026] The experimental results reveal that the composite film developed by the present invention has antibacterial properties and meets the requirements of easy-tear performance, and its comprehensive performance is relatively good, has practical application value, and can be used in dairy product packaging. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 It is a synthetic route for Schiff base coupling agents;
[0028] Figure 2 It is a synthetic route for Schiff base cross-linking agents;
[0029] Figure 3 The experimental results of antibacterial properties of composite membranes. DETAILED DESCRIPTION
[0030] Embodiment 1:
[0031] Preparation of Schiff base coupling agents, such as Figure 1 As shown, the synthesis process is as follows:
[0032] (1) Synthesizing a coumarin aldehyde monomer, wherein the specific synthesis method is as follows: using 7-hydroxycoumarin as a nucleophilic reagent, a nucleophilic substitution reaction is carried out between the bromine functional group of 2-bromoacetaldehyde and the hydroxyl functional group of 7-hydroxycoumarin to generate a coumarin aldehyde monomer, wherein the specific experimental steps are as follows: adding 3.2 g of 7-hydroxycoumarin and 50 mL of N,N-dimethylformamide into a three-necked flask, heating to 30° C. for dissolution for 30 min under nitrogen protection and mechanical stirring, then sequentially adding 1.5 mL of 2-bromoacetaldehyde and 10 mL of a potassium carbonate solution (prepared from 2.7 g of potassium carbonate and 20 mL of N,N-dimethylformamide) into the three-necked flask, heating to 70° C. for stirring and reacting for 10 h, filtering after cooling, washing with ethanol and deionized water in sequence, and vacuum drying to obtain a coumarin aldehyde monomer;
[0033] (2) Synthesizing a Schiff base coupling agent, wherein the specific synthesis method is as follows: utilizing the Schiff base reaction mechanism, the amino functional group of 3-aminopropyltrimethoxysilane and the carbonyl functional group of coumarin aldehyde monomer undergo a condensation reaction to generate a Schiff base coupling agent, wherein the specific experimental steps are as follows: adding 2.1 g of coumarin aldehyde monomer and 50 mL of anhydrous ethanol to a two-necked flask, heating to 30° C. and stirring until all the monomers are dissolved under mechanical stirring, cooling to room temperature, then dropping 2 mL of glacial acetic acid and 10 mL of 3-aminopropyltrimethoxysilane solution (prepared from 1.8 g of 3-aminopropyltrimethoxysilane and 10 mL of anhydrous ethanol) into the flask, heating to 85° C. and refluxing for 3 h, cooling and filtering, and recrystallizing with anhydrous ethanol and vacuum drying to obtain a Schiff base coupling agent;
[0034] The nuclear magnetic resonance hydrogen spectrum of the Schiff base coupling agent is characterized as follows: 1 H NMR(DMSO d6, 400MHz) δ: 0.80-0.83 (t, 2H), 1.68-1.74 (m, 2H), 3.14-3.16 (t, 2H), 3.57 (s, 9H), 4.73-4.74 (d, 2H), 6.29-6.94 (m, 3H), 7.43-7.45 (t, 1H, -N=CH-), 7.58-7.99 (m, 2H).
[0035] Embodiment 2:
[0036] Preparation of Schiff base crosslinkers, such as Figure 2 As shown, the synthesis process is as follows:
[0037] (1) Synthesizing a coumarin dialdehyde monomer, wherein the specific synthesis method is as follows: using 5,7-dihydroxycoumarin as a nucleophilic reagent, a bromine functional group of 2-bromoacetaldehyde reacts with a hydroxyl functional group of 5,7-dihydroxycoumarin to generate a coumarin dialdehyde monomer. The specific synthesis steps and synthesis reaction conditions refer to the synthesis experiment of the coumarin aldehyde monomer. The difference between the synthesis experiment of the coumarin aldehyde monomer and the synthesis experiment of the coumarin aldehyde monomer is that 1.8 g of 5,7-dihydroxycoumarin is used to replace 3.2 g of 7-hydroxycoumarin;
[0038] (2) Synthesizing a Schiff base crosslinking agent, wherein the specific synthesis method is as follows: utilizing the Schiff base reaction mechanism, the amino functional group of 3-aminopropyltrimethoxysilane and the carbonyl functional group of the coumarin dialdehyde monomer undergo a condensation reaction to generate a Schiff base crosslinking agent. The specific synthesis steps and synthesis reaction conditions refer to the synthesis experiment of the Schiff base coupling agent. The difference between the synthesis experiment of the Schiff base coupling agent and the synthesis experiment of the Schiff base coupling agent is that 2.6 g of the coumarin dialdehyde monomer replaces 2.1 g of the coumarin aldehyde monomer;
[0039] The nuclear magnetic resonance hydrogen spectrum of the Schiff base crosslinker is characterized as follows: 1 H NMR(DMSO d6, 400MHz) δ: 0.80-0.83 (t, 4H), 1.68-1.74 (m, 4H), 3.10-3.13 (t, 4H), 3.57 (s, 18H), 4.76-4.77 (dd, 4H), 6.32-6.55 (m, 3H), 7.43-7.48 (dt, 2H, -N=CH-), 8.10-8.12 (d, 1H).
[0040] Embodiment 3:
[0041] (1) preparing antibacterial agent I, wherein the preparation method is as follows: modifying hydroxylated nano zinc oxide with a Schiff base coupling agent to obtain antibacterial agent I, wherein the specific experimental steps are as follows: adding 1 g of Schiff base coupling agent, 3 g of hydroxylated nano zinc oxide and 50 mL of isopropanol into a round-bottom flask under nitrogen protection and mechanical stirring, heating to 25° C. and stirring for 6 h, then dropping 1 mL of ammonia water into the flask, continuing to stir for 18 h, washing with anhydrous ethanol, filtering, rotary evaporation and vacuum drying to obtain antibacterial agent I;
[0042] (2) preparing antibacterial agent II, the preparation method of which is: modifying hydroxylated nano zinc oxide with a Schiff base coupling agent and a Schiff base cross-linking agent to obtain antibacterial agent II, the specific experimental steps are: under nitrogen protection and mechanical stirring, adding 0.5 g of Schiff base coupling agent, 0.5 g of Schiff base cross-linking agent, 3 g of hydroxylated nano zinc oxide and 50 mL of isopropanol into a round-bottom flask, heating to 25°C and stirring for 6 h, then dropping 1 mL of ammonia water into the flask, continuing to stir and react for 18 h, washing with anhydrous ethanol, filtering, rotary evaporation, and vacuum drying to obtain antibacterial agent II;
[0043] The preparation method of hydroxylated nano zinc oxide is as follows: 20 g of zinc oxide nanoparticles and 200 mL of hydrogen peroxide aqueous solution (30 wt%) are added to a round-bottom flask, and the mixture is uniformly dispersed by ultrasonication for 10 min, and the mixture is heated to 105° C. and refluxed for 6 h under mechanical stirring, and then centrifuged at 5000 rpm for 5 min after cooling, and then washed with deionized water for 3 times, and finally dried under vacuum at 80° C. for 5 h to obtain hydroxylated nano zinc oxide;
[0044] The zinc oxide nanoparticles were purchased from Changzhou Konada New Material Technology Co., Ltd., and the model number was KND-NX10.
[0045] Embodiment 4:
[0046] (1) preparing composite membrane I, comprising the following steps:
[0047] Step 1, preparing a BOPE surface layer: adding 45g of low-density polyethylene resin and 3g of antibacterial agent I to a twin-screw extruder preheated to 140°C, blending, melting, and extruding through the twin-screw extruder, and then successively stretching them longitudinally and then transversely, the temperature during longitudinal stretching is 80°C, the stretching ratio is 5 times, the temperature during transverse stretching is 150°C, the stretching ratio is 6 times, and finally hot pressing is performed at 140°C to obtain a BOPE surface layer;
[0048] Among them, the process parameters of the twin-screw extruder corresponding to the BOPE surface layer are set as follows: the temperatures of zones 1-3 are 110°C, 140°C, and 160°C, respectively, and the rotation speed is 30r / min;
[0049] Step 2, preparing a barrier intermediate layer: adding 10g of ethylene-vinyl alcohol copolymer resin and 15g of low-density polyethylene resin into a twin-screw extruder preheated to 170°C, blending, melting and extruding through the twin-screw extruder, cutting them with a pelletizer to obtain 1-5mm particles, and then directly adding them into a casting machine preheated to 170°C, casting into a film, and obtaining a barrier intermediate layer;
[0050] Among them, the process parameters of the twin-screw extruder corresponding to the barrier middle layer are set as follows: the temperatures of zones 1-3 are 160°C, 185°C, and 200°C, respectively, and the rotation speed is 40r / min;
[0051] Step 3, preparing the PE inner layer: adding 45g of low-density polyethylene resin and 3g of antibacterial agent I into a twin-screw extruder preheated to 140°C, blending, melting and extruding through the twin-screw extruder, cutting them with a pelletizer to obtain 1-5mm particles, and then directly adding them to a casting machine preheated to 140°C, casting into a film, and obtaining a PE inner layer;
[0052] Among them, the process parameters of the twin-screw extruder corresponding to the PE inner layer were set as follows: the temperatures of zones 1-3 were 110°C, 140°C, and 160°C, respectively, and the rotation speed was 30 r / min;
[0053] Step 4, preparing composite film I: using a high-speed solvent-free composite machine to bond the BOPE surface layer, the barrier middle layer and the PE inner layer together, the composite speed is 400m / min, the composite temperature is 45°C, the cooling temperature is 25°C, the composite pressure is 0.4Mpa, and the gluing pressure is 0.5Mpa, to obtain a composite film I with a thickness of 100μm;
[0054] Among them, the low-density polyethylene resin was purchased from CNOOC Shell Petrochemical Co., Ltd., with the specifications of 2420H, Mn~180000, MFR 2.0~2.5g / 10min; the ethylene-vinyl alcohol copolymer resin was purchased from Dongguan Kaisi Li Plastic Raw Materials Co., Ltd., with the specifications of E105B, Mn~10000, ethylene content 44%.
[0055] (2) Preparation of composite membrane II: Antimicrobial agent II was used instead of antimicrobial agent I, referring to the preparation steps and experimental conditions of composite membrane I to prepare composite membrane II.
[0056] Performance Testing:
[0057] (1) Select the trouser tear method and test the tear strength of the sample according to GB / T 16578.1-2008. The specific test steps are as follows: cut a 75 mm long straight line incision in the middle of the 50 mm dimension of a 150 mm × 50 mm sample, then clamp it on an Instron 55650000 material testing machine, select the tear strength test item for the test, record the longitudinal and transverse tear strengths of the sample, and calculate the average tear force of the sample;
[0058] (2) The tensile strength of the sample was tested using an Instron 5565 universal material testing machine. The specific test steps were as follows: a 150 mm × 20 mm sample was fixed on the material testing machine, and a tensile test was performed at a tensile rate of 5 mm / min, and the longitudinal and transverse tensile strengths of the sample were recorded;
[0059] (3) The antibacterial performance test was carried out using an MJ-250I mold incubator. The specific test steps were as follows: the sample was cut into a disc with a diameter of 6 mm and irradiated with ultraviolet light for 2 h to fully sterilize it. Then, 100 μL of bacterial solution (concentration of 1.0×10 6 CFU / mL), place the sterile sample flat in the culture medium, place it in an incubator at 37°C and invert it for 24 hours, and observe the diameter of the inhibition zone;
[0060] The bacterial liquid was ATCC6538 Staphylococcus aureus and ATCC25922 Escherichia coli purchased from Shanghai Luwei Technology Co., Ltd.
[0061] (4) The oxygen permeability performance test of the sample was carried out in accordance with GB / T 1038-2000. The specific test steps are as follows: a 30 cm round sample was placed in a glass desiccator at an ambient temperature of 25°C and anhydrous calcium chloride was used as a desiccant for 72 hours. After that, the sample was tested using a Y110 oxygen permeability tester;
[0062] (5) Test the hygienic properties of the samples according to GB / T 5009.60-2003 “Analytical methods for hygienic standards of polyethylene, polystyrene and polypropylene moldings for food packaging”;
[0063] The above experimental results are shown in Tables 1-3 below.
[0064] Table 1 Test results of tearing properties and mechanical properties of composite films
[0065]
[0066] Table 2 Antibacterial and barrier test results of composite films
[0067]
[0068]
[0069] Table 3 Hygienic performance test results of composite membrane
[0070]
[0071] Note: The physical and chemical indicators of the experimental results are based on GB / T 5009.58-2003 "Analysis Methods for Hygienic Standards of Polyethylene Resins for Food Packaging";
[0072] According to the antibacterial performance test data in Table 2, Figure 3 , through comprehensive analysis of the above experimental results, we can draw the following conclusions:
[0073] (1) The present invention refers to the national standards and the requirements of enterprise users. The tearing force of the sample tested by the trouser method should be ≤2N. From the test results in Table 1, it can be seen that the composite films prepared by the present invention meet the requirements of easy tearing performance;
[0074] (2) Composite membrane I and composite membrane II both showed significant inhibitory effects on Staphylococcus aureus and Escherichia coli, that is, composite membrane I and composite membrane II had antibacterial properties;
[0075] (3) The oxygen permeability of three-layer film used in dairy product packaging is required to be less than 2.47×10 -2 cm 3 / (m 2 ·24h·Pa), it can be seen from the test results in Table 2 that the composite films prepared by the present invention meet the requirements for use of dairy product packaging;
[0076] (4) The sanitation of the composite films I and II prepared by the present invention meets the requirements of national standards and can be used in dairy product packaging.
Claims
1. A method for preparing an easy-to-tear composite packaging material for dairy products, It is characterized in that The following steps are involved: Step 1, preparing a composite antibacterial agent, wherein the preparation method comprises: synthesizing a Schiff base coupling agent, and using the Schiff base coupling agent to perform surface modification on hydroxylated nano zinc oxide particles; Step 2: Using low-density polyethylene resin and composite antibacterial agent as raw materials, blending, melting, and extruding through a twin-screw extruder, and performing longitudinal and then transverse stretching treatment, and hot pressing and shaping to obtain a BOPE surface layer; Using ethylene-vinyl alcohol copolymer resin and low-density polyethylene resin as raw materials, they are blended, melted, extruded and pelletized through a twin-screw extruder, and then cast into a film to obtain a barrier intermediate layer; Low-density polyethylene resin and composite antibacterial agent are used as raw materials, blended, melted, extruded and pelletized through a twin-screw extruder, and then cast into a film to obtain a PE inner layer; Step three, using a high-speed solvent-free composite process to bond the BOPE surface layer, the barrier middle layer and the PE inner layer to obtain a composite film, which is an easy-to-tear composite packaging material for dairy products.
2. The method for preparing the easy-to-tear composite packaging material for dairy products according to claim 1, It is characterized in that The preparation method of the composite antibacterial agent comprises the following steps: synthesizing a Schiff base coupling agent and a Schiff base crosslinking agent, and using the Schiff base coupling agent and the Schiff base crosslinking agent to perform surface modification on hydroxylated nano zinc oxide particles.
3. The method for preparing the easy-to-tear composite packaging material for dairy products according to claim 2, It is characterized in that The preparation method of the Schiff base coupling agent is: Step S3-1: using 7-hydroxycoumarin as a nucleophilic reagent, a bromine functional group of 2-bromoacetaldehyde reacts with a hydroxyl functional group of 7-hydroxycoumarin to generate a coumarin aldehyde monomer; Step S3-2: using the Schiff base reaction mechanism, the amino functional group of 3-aminopropyltrimethoxysilane and the carbonyl functional group of the coumarin aldehyde monomer undergo a condensation reaction to generate a Schiff base coupling agent.
4. The method for preparing the easy-to-tear composite packaging material for dairy products according to claim 2, It is characterized in that The preparation method of the Schiff base crosslinking agent is: Step S4-1: using 5,7-dihydroxycoumarin as a nucleophilic reagent, a bromine functional group of 2-bromoacetaldehyde and a hydroxyl functional group of 5,7-dihydroxycoumarin undergo a nucleophilic substitution reaction to generate a coumarin dialdehyde monomer; Step S4-2: using the Schiff base reaction mechanism, the amino functional group of 3-aminopropyltrimethoxysilane and the carbonyl functional group of the coumarin dialdehyde monomer undergo a condensation reaction to generate a Schiff base crosslinking agent.
5. The method for preparing the easily tearable composite packaging material for dairy products according to claim 1, It is characterized in that The preparation process parameters of the composite film in step three are set as follows: composite speed of 300-500 m / min, composite temperature of 40-50° C., cooling temperature of 20-30° C., composite pressure of 0.3-0.5 MPa, and gluing pressure of 0.4-0.6 MPa.
6. An easy-to-tear composite packaging material for dairy products prepared according to the method according to any one of claims 1 to 5, It is characterized in that The thickness of the easily tearable composite packaging material for dairy products is 80 to 200 μm.
7. The easily tearable composite packaging material for dairy products according to claim 6, It is characterized in that The average tearing force of the easy-to-tear composite packaging material for dairy products is 0.9-1.2N.
8. The easily tearable composite packaging material for dairy products according to claim 6, It is characterized in that The easy-to-tear composite packaging material for dairy products has an antibacterial effect, and the bacteria are Escherichia coli or Staphylococcus aureus.
Citation Information
Patent Citations
Preparation method of inorganic-multiple organic composite antibacterial agent and application thereof
CN111410771A
High-barrier composite film and preparation method thereof
CN113524843A
Barrier type polyvinyl single-material composite antibacterial film and preparation method thereof
CN117141077A
7-indazolyl-3-phenyl-coumarins
GB1200852A
Wrapping sheet
JP1994155682A