Preparation method of molybdenum carbide nano frame material and prepared material

By using metal organic frame materials as precursors and combined with high-temperature carbonization technology, highly dispersed molybdenum carbide nanoframe materials are prepared, which solves the problems of large size and difficult to control the morphology of molybdenum carbide in the prior art, and realizes supercapacitors and capacitors Excellent electrochemical performance and efficient capacitive desalting in deionized devices.

CN118877892AActive Publication Date: 2024-11-01HEBEI AGRICULTURAL UNIV.
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410911127.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-11-01
Estimated Expiration
2044-07-09

AI Technical Summary

Technical Problem

The existing molybdenum carbide preparation method is complex, requiring high reaction temperature and energy consumption. The prepared material has a low specific surface area, large particle size and uneven particle size distribution, and its morphology is difficult to control, which limits its use in supercapacitors and capacitor deionized devices. Application performance in .

Method used

Metal organic framework materials (MOFs) are used as precursors, and highly dispersed molybdenum carbide nanoframe materials are prepared through ion exchange and high-temperature carbonization process, which overcomes the difficulties in particle size and morphology control. The specific steps include hydrothermal reaction to prepare the precursor composite and carbonize at a high temperature under a nitrogen atmosphere of 700 to 900°C.

Benefits of technology

A highly dispersed MoC and Mo2C two-phase crystal structure and rich pore structure are achieved, which improves the conductivity and electrochemical performance of the material. As an electrode material, it shows excellent electrochemical performance and capacitance in supercapacitors and capacitor deionized devices. Desalination efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118877892A_ABST
    Figure CN118877892A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a molybdenum carbide nano frame material. The preparation method comprises the following steps: respectively dissolving first transition metal acetate, dimethylimidazole and cetyltrimethylammonium bromide in water to prepare a solution and a precursor; adding a second transition metal acetate solution, a dimethylimidazole solution and a hexadecyl trimethyl ammonium bromide solution into the precursor to prepare a precursor compound; then dissolving the precursor compound and molybdate in a dimethylformamide solution to prepare a molybdate compound; and finally, carrying out high-temperature carbonization on the molybdate compound in a nitrogen atmosphere at 700-900 DEG C to obtain the molybdenum carbide nano-frame material. The material has a highly dispersed MoC and Mo2C two-phase crystal structure, a rich pore structure and good conductivity, and shows excellent electrochemical performance and capacitance desalination efficiency when being applied to a supercapacitor and a capacitive deionization device as an electrode material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the preparation of transition metal carbides, and in particular to a preparation method of a highly dispersed molybdenum carbide nanoframe material and the prepared material. Background Art

[0002] As a type of transition metal carbide, molybdenum carbide has the advantages of high conductivity and good structural stability. It is widely used in chemical engineering, electronic devices, aerospace, energy conversion and storage, and electrocatalysis. At present, the main methods for preparing molybdenum carbide are chemical vapor deposition, programmed temperature method, and carbon thermal reduction method. However, these methods usually have complex preparation processes, require high reaction temperatures and more energy consumption, and the prepared molybdenum carbide has a low specific surface area, large particle size and uneven particle size distribution, and difficult to control morphology. In recent years, researchers have found that using molybdenum-containing metal organic framework materials (MOFs) as precursors, high-temperature carbonization process can achieve the preparation of nano-molybdenum carbide. Although the molybdenum carbide particles prepared by this method are small, it is limited by the small number of molybdenum-containing MOFs and the single structure, which limits the improvement of its practical application performance. Summary of the invention

[0003] The purpose of the present invention is to provide a method for preparing a molybdenum carbide nanoframe material. The molybdenum carbide prepared by the method has a highly dispersed MoC and Mo2C two-phase crystal structure, a rich pore structure and good conductivity. The molybdenum carbide is applied as an electrode material to supercapacitors and capacitive deionization devices, and exhibits excellent electrochemical properties and capacitive desalination efficiency.

[0004] In order to solve the above problems, the present invention adopts the following technical solutions:

[0005] A method for preparing a molybdenum carbide nanoframe material comprises the following steps:

[0006] Step S1: dissolving a first transition metal acetate, dimethylimidazole and hexadecyltrimethylammonium bromide in water to prepare a solution, mixing the solution and performing a hydrothermal reaction at 110-130° C. for 3-5 hours to obtain a precursor, wherein the molar ratio of the first transition metal acetate to dimethylimidazole and hexadecyltrimethylammonium bromide is 2:5:0.6 respectively;

[0007] Step S2: adding a second transition metal acetate solution, a dimethylimidazole solution and a hexadecyltrimethylammonium bromide solution to the precursor prepared in step S1 in sequence, and subjecting the mixture to a hydrothermal reaction at 110-130° C. for 2-3 hours to obtain a precursor complex, wherein the mass ratio of the second transition metal acetate to the precursor is 5:4, and the molar ratios of the second transition metal acetate to the dimethylimidazole and the hexadecyltrimethylammonium bromide are 0.5:1.25:0.15 in sequence;

[0008] Step S3: dissolving the precursor complex prepared in step S2 and molybdate in a dimethylformamide solution, stirring and hydrothermally reacting at 110-130° C. for 5-7 hours to obtain a molybdate complex, wherein the mass ratio of the precursor complex to the molybdate is 1:1-2;

[0009] Step S4: carbonizing the molybdate complex prepared in step S3 at a high temperature of 700-900° C. in a nitrogen atmosphere for 3 h to obtain a molybdenum carbide nanoframe material.

[0010] Preferably, the first transition metal acetate is one of zinc acetate dihydrate and cobalt acetate tetrahydrate, and the precursor is one of T-ZIF-8 formed by the reaction of zinc and dimethylimidazole or T-ZIF-67 formed by the reaction of cobalt and dimethylimidazole.

[0011] Preferably, the second transition metal acetate is one of zinc acetate dihydrate and cobalt acetate tetrahydrate, and the complex is one of zinc / cobalt complex T-ZIF-8 / ZIF-67, cobalt / zinc complex T-ZIF-67 / ZIF-8, and zinc / zinc complex T-ZIF-8 / ZIF-8.

[0012] Preferably, the molybdate is one of ammonium molybdate and sodium molybdate dihydrate.

[0013] Another object of the present invention is to provide a molybdenum carbide nanoframe material prepared by the above preparation method.

[0014] In the present invention, MOFs are used as precursors, and highly dispersed molybdenum carbide nanoframe materials are prepared by combining ion exchange with high-temperature carbonization. This method overcomes the disadvantages of large molybdenum carbide particles, uneven particle size distribution, and difficult morphology control prepared by conventional methods, and can avoid the problem of poor dispersion due to agglomeration of molybdenum carbide particles. The molybdenum carbide nanoframe materials prepared by the present invention are assembled into supercapacitors and capacitor deionization devices as electrode materials. At a current density of 0.5A g -1 When the electrolyte is 1 mol L -1 The material has a capacitance of up to 185.4 F g -1 ; 500mg L -1 The desalination capacity of CDI at 1.4 V is 73.6 mg g -1 , the desalination capacity after 50 cycle tests remained at 92.1%. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 The scanning electron microscope image (A), transmission electron microscope image (B), high-magnification transmission electron microscope image (C) and carbon / molybdenum element mapping image (DF) of the molybdenum carbide nanoframe material;

[0016] Figure 2 The X-ray diffraction pattern of molybdenum carbide nanoframe material and the standard MoC and Mo2C spectra;

[0017] Figure 3 This is the Raman spectrum of MoC nanoframe material;

[0018] Figure 4 X-ray photoelectron spectra of MoC nanoframe materials: (A) full energy spectrum, (B) Mo 3d spectrum;

[0019] Figure 5 (A) Nitrogen adsorption-desorption isotherm and (B) pore size distribution of MoC nanoframe materials;

[0020] Figure 6 Cyclic voltammetry curve of supercapacitor made of molybdenum carbide nanoframe material (electrolyte 1 mol / L sodium chloride solution);

[0021] Figure 7 This is the charge and discharge curve of the supercapacitor made of molybdenum carbide nanoframe material (electrolyte 1 mol / L sodium chloride solution);

[0022] Figure 8 This is a graph showing the specific capacitance performance of MoC nanoframe materials;

[0023] Fig. 9 This is the electrochemical impedance curve of the MoC nanoframe material;

[0024] Fig.10 The following are photos of the device and components of MoC-based capacitive deionization (CDI);

[0025] Fig.11 (A) Curve of desalination amount changing with time and (B) Ragone curve of desalination amount and desalination rate based on molybdenum carbide CDI;

[0026] Fig.12 The desalination capacity under different NaCl concentrations based on MoC nanoframe material CDI;

[0027] Fig.13 The desalination capacity at different voltages based on MoC nanoframe material CDI;

[0028] Fig.14 This is the 50-cycle stability curve of CDI based on molybdenum carbide nanoframe material. DETAILED DESCRIPTION

[0029] The present invention will be further described below by means of specific examples.

[0030] Example 1 Preparation method of molybdenum carbide nanoframe material 1

[0031] First, 0.439 g (2.0 mmol) of zinc acetate dihydrate, 4.105 g (5.0 mmol) of dimethylimidazole and 0.217 g (0.6 mmol) of hexadecyltrimethylammonium bromide (CTAB) were dissolved in deionized water to prepare solutions, and the three solutions were mixed and stirred for 0.5 hours. The mixed solution was transferred to an autoclave, heated at 120°C for 4 hours, centrifuged and washed with ethanol three times, and vacuum dried to obtain a precursor (T-ZIF-8).

[0032] Then, 0.125 g (0.5 mmol) of cobalt acetate tetrahydrate was dissolved in 20 ml of aqueous solution, 100 mg of precursor T-ZIF-8 was added to the above solution and ultrasonically dispersed for 10 minutes. 1.03 g (1.25 mmol) of dimethylimidazole and 0.054 g (0.15 mmol) of CTAB were dissolved in 10 ml of deionized water, added to the cobalt / T-ZIF-8 dispersion solution, stirred and reacted at 120°C in an autoclave for 2 hours, and the solid obtained was centrifuged and washed with ethanol. After vacuum drying, a purple composite (T-ZIF-8 / ZIF-67) was obtained.

[0033] Subsequently, 100 mg of the prepared T-ZIF-8 / ZIF-67 complex was added to 15 ml of DMF solution and dispersed by ultrasound. 200 mg (0.16 mmol) of ammonium molybdate tetrahydrate was added to the above dispersion and stirred for 10 minutes, transferred to an autoclave, and reacted at 120 degrees Celsius for 6 hours. After cooling to room temperature, a gray-purple molybdate complex (T-ZIF-8 / ZIF-67 / MoO4) was obtained, and the product was separated by centrifugation, washed with ethanol, and then dried.

[0034] Finally, the molybdate complex was pyrolyzed at 800 degrees Celsius in nitrogen for 3 hours to obtain a nano-framework structured molybdenum carbide material.

[0035] In this embodiment, the scanning electron microscope image, transmission electron microscope image, high-magnification transmission electron microscope image and carbon / molybdenum element mapping image of the molybdenum carbide nanoframe material are shown as follows: Figure 1 As shown in Figure AF, the synthesized molybdenum carbide has a nanoframe structure morphology, and the MoC / Mo2C two-phase crystals are uniformly dispersed in the MOF-derived carbon matrix. Figure 2 As shown, it is further explained that the synthesized molybdenum carbide nanoframe material has a two-phase crystal structure of MoC (JCPDS No.45-1015) and Mo2C (JCPDS No.35-0787). Figure 3 The Raman spectrum shows that the proportion of graphitized carbon (G peak) in the MoC nanoframe material is slightly higher than that of amorphous carbon (D peak). Figure 4The X-ray photoelectron spectroscopy (XPS) of the MoC nanoframe material shows that the Mo element is successfully embedded in the material ( Figure 4 A), High-resolution XPS spectra of Mo 3d region ( Figure 4 Two pairs of peaks are observed in B). The first pair of peaks: Mo 3d 5 / 2 Peak at 228.88eV, Mo 3d 3 / 2 The peaks are at 231.95 eV, which can be attributed to Mo-Mo or Mo-C bonds; the second pair of peaks is located at higher binding energy (Mo 3d 5 / 2 At 232.98eV, Mo 3d 3 / 2 At 236.01 eV), it is a Mo-O bond. The nitrogen adsorption-desorption isotherm is as follows Figure 5 As shown in A, a hysteresis loop appears between the relative pressure of 0.4 and 0.9, indicating that the MoC nanoframe material has mesoporous structural characteristics, which is consistent with its mesopore pore size distribution curve ( Figure 5 B).

[0036] Example 2 Preparation method of molybdenum carbide nanoframe material 2

[0037] First, 0.439 g (2.0 mmol) of zinc acetate dihydrate, 4.105 g (5.0 mmol) of dimethylimidazole and 0.217 g (0.6 mmol) of CTAB were dissolved in deionized water to prepare solutions, and the three solutions were mixed and stirred for 0.5 hours. The mixed solution was transferred to an autoclave, heated at 110° C. for 5 hours, centrifuged and washed with ethanol, and vacuum dried to obtain a precursor (T-ZIF-8).

[0038] Then, 0.125 g (0.5 mmol) of cobalt acetate tetrahydrate was dissolved in 20 ml of aqueous solution, 100 mg of the precursor T-ZIF-8 was added to the above solution and ultrasonically dispersed for 10 minutes. Then 1.03 g (1.25 mmol) of dimethylimidazole and 0.054 g (0.15 mmol) of CTAB were dissolved in 10 ml of deionized water, added to the cobalt / T-ZIF-8 dispersion solution, stirred and reacted at 110°C in an autoclave for 3 hours, the solid was centrifuged and washed with ethanol, and a purple complex (T-ZIF-8 / ZIF-67) was obtained after vacuum drying.

[0039] Subsequently, 100 mg of the prepared T-ZIF-8 / ZIF-67 complex was added to 15 ml of DMF solution and ultrasonically dispersed. 100 mg (0.08 mmol) of ammonium molybdate tetrahydrate was added to the above dispersion and stirred for 10 minutes, transferred to an autoclave, and reacted at 130 degrees Celsius for 5 hours. After cooling to room temperature, the molybdate complex T-ZIF-8 / ZIF-67 / MoO4 with different proportions was obtained in gray-purple color, centrifuged, washed with ethanol and dried.

[0040] Finally, the material was pyrolyzed at 700 degrees Celsius under nitrogen for 4 hours to obtain a molybdenum carbide material with a nano-frame structure.

[0041] Example 3 Preparation method of molybdenum carbide nanoframe material 3

[0042] First, 0.498 g (2.0 mmol) of cobalt acetate tetrahydrate, 4.105 g (5.0 mmol) of dimethylimidazole and 0.217 g (0.6 mmol) of CTAB were dissolved in deionized water to prepare solutions, and the three solutions were mixed and stirred for 0.5 hours. The mixed solution was transferred to an autoclave, reacted at 130 degrees Celsius for 3 hours, and the product was collected by centrifugation, washed with ethanol 3 times, and then vacuum dried to obtain a purple precursor (T-ZIF-67).

[0043] Then, 0.125 g (0.5 mmol) of cobalt acetate tetrahydrate was dissolved in 20 ml of aqueous solution, 100 mg of the precursor T-ZIF-67 was added to the above solution and ultrasonically dispersed for 10 minutes. Then 1.03 g (1.25 mmol) of dimethylimidazole and 0.054 g (0.15 mmol) of CTAB were dissolved in 10 ml of deionized water, added to the cobalt / T-ZIF-67 dispersion solution, stirred and reacted at 130°C in an autoclave for 2 hours, centrifuged and washed with ethanol, and vacuum dried to obtain a purple complex (T-ZIF-67 / ZIF-67).

[0044] Subsequently, 100 mg of the prepared T-ZIF-67 / ZIF-67 complex was added to 15 ml of DMF solution and ultrasonically dispersed. 200 mg (0.16 mmol) of ammonium molybdate tetrahydrate was added to the above dispersion and stirred for 10 minutes, transferred to an autoclave, and reacted at 110 degrees Celsius for 7 hours. After cooling to room temperature, the obtained molybdate complex T-ZIF-67 / ZIF-67 / MoO4 was centrifuged, washed with ethanol, and then dried.

[0045] Finally, T-ZIF-67 / ZIF-67 / MoO4 was pyrolyzed at 900 degrees Celsius in nitrogen for 2 hours to obtain a nano-framework structured molybdenum carbide material.

[0046] Example 4 Preparation method of molybdenum carbide nanoframe material 4

[0047] First, 0.439 g (2.0 mmol) of zinc acetate dihydrate, 4.105 g (5.0 mmol) of dimethylimidazole and 0.217 g (0.6 mmol) of CTAB were dissolved in deionized water to prepare solutions, and the three solutions were mixed and stirred for 0.5 hours. The mixed solution was transferred to an autoclave, reacted at 120 degrees Celsius for 4 hours, centrifuged and washed with ethanol, and then vacuum dried to obtain a white precursor (T-ZIF-8).

[0048] Then, 0.110 g (0.5 mmol) of zinc acetate dihydrate was dissolved in 20 ml of aqueous solution, 100 mg of the precursor T-ZIF-8 was added to the above solution and ultrasonically dispersed for 10 minutes. Then 1.03 g (1.25 mmol) of dimethylimidazole and 0.054 g (0.15 mmol) of CTAB were dissolved in 10 ml of deionized water, added to the zinc / T-ZIF-8 dispersion solution, stirred and reacted at 120°C in an autoclave for 2 hours, centrifuged and washed with ethanol, and vacuum dried to obtain a white composite (T-ZIF-8 / ZIF-8).

[0049] Subsequently, 100 mg of T-ZIF-8 / ZIF-8 complex was added to 15 ml of DMF solution and ultrasonically dispersed. 200 mg (0.16 mmol) of ammonium molybdate tetrahydrate was added to the above dispersion and stirred for 10 minutes, transferred to an autoclave, and reacted at 120 degrees Celsius for 6 hours. After cooling to room temperature, the molybdate complex T-ZIF-8 / ZIF-8 / MoO4 was centrifuged, washed with ethanol, and then dried.

[0050] Finally, T-ZIF-8 / ZIF-8 / MoO4 was pyrolyzed at 800 degrees Celsius under nitrogen for 3 hours to obtain molybdenum carbide material.

[0051] Performance test of molybdenum carbide nanoframe material

[0052] 2 mg of molybdenum carbide prepared in Example 1 was applied as electrode material to a 1×2 cm 2 The conductive graphite paper was used as the test electrode, and a supercapacitor was assembled with a platinum wire counter electrode and an Ag / AgCl reference electrode and then charged at 1 mol L -1 The capacitance performance test was carried out in sodium chloride solution. The test results are as follows Figures 6 to 9 As shown in Figure 2, the MoC nanoframe material exhibits a high specific capacitance (current density of 0.5 A g -1 When the capacitance is 185.4F g -1 ), fast charge and discharge characteristics and good conductivity. 16 mg of molybdenum carbide was used as the electrode material and evenly coated on a 2×2 cm 2Conductive graphite paper was used as the CDI cathode, and the CDI anode was prepared by the same method to assemble a symmetrical capacitive deionization CDI device ( Fig.10 ) to perform performance testing, the test results are as follows Figures 11 to 14 As shown. The material is 500 mg L -1 The salt adsorption capacity of sodium chloride solution at 1.4 V is 73.6 mg g -1 ( Fig.11 A) From Fig.11 The Ragone curve of desalination amount and desalination rate of B shows that the molybdenum carbide nanoframe material has a fast desalination rate. Fig.12 and Fig.13 It is further shown that the CDI of the MoC nanoframe material increases with the increase of the NaCl solution concentration and the applied voltage. -1 The cyclic desalination experiment in sodium chloride solution showed that the prepared material has good cyclic stability, and the desalination capacity after 50 cycles remained at 92.1% ( Fig.14 ).

[0053] The above embodiments are merely illustrative of the concept and implementation of the present invention, and are not intended to limit the concept and implementation of the present invention. Under the concept of the present invention, technical solutions that have not been substantially changed are still within the scope of protection.

Claims

1. A method for preparing a molybdenum carbide nanoframe material, characterized in that The steps include: Step S1: dissolving a first transition metal acetate, dimethylimidazole and hexadecyltrimethylammonium bromide in water to prepare a solution, mixing the solution and performing a hydrothermal reaction at 110-130° C. for 3-5 hours to obtain a precursor, wherein the molar ratio of the first transition metal acetate to dimethylimidazole and hexadecyltrimethylammonium bromide is 2:5:0.6 respectively; Step S2: adding a second transition metal acetate solution, a dimethylimidazole solution and a hexadecyltrimethylammonium bromide solution to the precursor prepared in step S1, and subjecting the mixture to a hydrothermal reaction at 110-130° C. for 2-3 hours to obtain a precursor complex, wherein the mass ratio of the second transition metal acetate to the precursor is 5:4, and the molar ratios of the second transition metal acetate to the dimethylimidazole and the hexadecyltrimethylammonium bromide are 0.5:1.25:0.15, respectively; Step S3: dissolving the precursor complex prepared in step S2 and molybdate in a dimethylformamide solution, stirring and hydrothermally reacting at 110-130° C. for 5-7 hours to obtain a molybdate complex, wherein the mass ratio of the precursor complex to the molybdate is 1:1-2; Step S4: carbonizing the molybdate complex prepared in step S3 at 700-900° C. in an inert atmosphere for 2-4 hours to obtain a molybdenum carbide nanoframe material.

2. The method for preparing the molybdenum carbide nanoframe material according to claim 1, characterized in that: The first transition metal acetate is one of zinc acetate dihydrate and cobalt acetate tetrahydrate.

3. The method for preparing the molybdenum carbide nanoframe material according to claim 1, characterized in that: The second transition metal acetate is one of zinc acetate dihydrate and cobalt acetate tetrahydrate.

4. The method for preparing the molybdenum carbide nanoframe material according to claim 1, characterized in that: The molybdate is one of ammonium molybdate and sodium molybdate dihydrate.

5. The method for preparing the molybdenum carbide nanoframe material according to claim 1, characterized in that: The inert atmosphere is nitrogen or argon.

6. The method for preparing the molybdenum carbide nanoframe material according to claim 1, characterized in that: In the step S1, the first transition metal acetate, dimethyl imidazole and hexadecyl trimethyl ammonium bromide are dissolved in water to prepare solutions, and after mixing, the solutions are subjected to hydrothermal reaction at 120° C. for 4 hours to obtain a precursor; In the step S2, a second transition metal acetate solution, a dimethyl imidazole solution and a hexadecyl trimethyl ammonium bromide solution are sequentially added to the precursor prepared in the step S1, and a hydrothermal reaction is carried out at 120° C. for 2 hours to obtain a precursor composite; In the step S3, the precursor complex prepared in step S2 and molybdate are dissolved in a dimethylformamide solution, stirred and hydrothermally reacted at 120° C. for 6 hours to obtain a molybdate complex, wherein the mass ratio of the precursor complex to the molybdate is 1:1-2; Step S4: The molybdate complex prepared in step S3 is carbonized at 800° C. in an inert atmosphere for 3 hours to obtain a molybdenum carbide nanoframe material.

7. A molybdenum carbide nanoframe material, characterized in that It is prepared by the preparation method according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Molybdenum disulfide / carbon composite hydrogen evolution electro-catalyst and preparation method thereof

    CN108441884A

  • 1T-MoS2-modified ZnCoS solid solution hollow dodecahedral nanocomposite and preparation method and application thereof

    CN109806888A

  • Preparation methods of ZIF-8 nanosheet crystals and ultrathin film thereof

    CN111533921A

  • Carbon-separated Ultrafine Nano Tungsten Carbide Material And Preparation Method And Use Thereof

    US20150210554A1