Production method of high-dispersion large-specific-surface-area zinc oxide

Through the reaction of acid zinc sulfate and barium peroxide, combined with sodium hydroxide and calcination and blasting steps, the existing zinc oxide preparation methods are solved, and the production of zinc oxide with high efficiency and low cost is achieved with high dispersion and large specific surface area of ​​zinc oxide. , has high purity and high dispersion characteristics.

CN118877926AInactive Publication Date: 2024-11-01ANHUI JINHUA ZINC OXIDE CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411376770.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-11-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing preparation method for large specific surface area zinc oxide is complex, using organic solvents and inert gases, which is costly and not suitable for industrial production.

Method used

Acid zinc sulfate aqueous solution is used to react with barium peroxide under ice water bath conditions, and then sodium hydroxide solution is added, and after filtration, washing, drying and calcining and blasting, a high-dispersion large specific surface area zinc oxide is obtained.

Benefits of technology

实现了高纯度、比表面积大的纳米氧化锌生产,操作简便,污染小,成本低,产量高,并且副产物沉淀重晶石粉增加了经济效益。

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the technical field of zinc oxide materials, and particularly relates to a production method of high-dispersion large-specific-surface-area zinc oxide, which comprises the following steps of: adding barium peroxide into an acidic zinc sulfate aqueous solution to react, and performing filter pressing, washing and drying by using a sodium hydroxide solution to obtain the high-dispersion large-specific-surface-area zinc oxide. The yellow solid is rapidly converted into heat energy through the calcining heating effect, self-oxidation and blasting can be rapidly carried out, the high-purity and large-specific-surface-area nano-zinc oxide is obtained, the method has the advantages of being high in yield, easy and convenient to operate, small in pollution and the like, and a by-product, namely precipitated barite powder can be obtained. The economic benefit of the method is increased, and the characteristics of high specific surface area, high surface energy, high dispersion and the like are obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of zinc oxide materials, in particular to a method for producing highly dispersed zinc oxide with a large specific surface area. Background Art

[0002] Due to its large specific surface area and high surface activity, zinc oxide can improve the compression permanent deformation of rubber, especially EPDM. Due to its small specific gravity and large number of particles, it has good dispersibility. In addition, the method of increasing the specific surface area of ​​zinc oxide particles can expose more ZnO molecules, so that more zinc oxide can interact with gastrointestinal tissues and microbial flora, which can improve the effect of zinc oxide. In addition, zinc oxide has also attracted much attention due to its high specific surface area, low toxicity, good biocompatibility, and biodegradability. It is an important material for biomedical and biophilic systems. On May 03, 2019, CN109704388A disclosed a method for preparing zinc oxide with a large specific surface area, but its synthesis method is complicated, using a large amount of organic solvents such as butanol and hexane, using inert gases, and the source of raw materials is limited and the cost is high. For example, dimethyl zinc is a volatile polymerization catalyst, which is expensive and cannot be used for industrial production of zinc oxide. At present, only a small amount is used for CVD zinc oxide film growth. In order to solve the above problems, those skilled in the art are in urgent need of developing a production method of highly dispersed zinc oxide with a large specific surface area and its application to meet the existing market demand and performance requirements. Summary of the invention

[0003] In view of the above problems, the present invention aims to provide a method for producing highly dispersed zinc oxide with a large specific surface area.

[0004] A method for producing highly dispersed zinc oxide with a large specific surface area comprises the following steps: The first step is to prepare a zinc sulfate aqueous solution with zinc sulfate, and adjust the pH value thereof to 0.5-1 with dilute sulfuric acid to obtain a 55-60 g / L acidic zinc sulfate aqueous solution; the second step is to premix barium peroxide with 0°C ice water to form a barium peroxide paste; the third step is to immediately mix the obtained barium peroxide paste with the acidic zinc sulfate aqueous solution in a 0°C ice water bath for 10-15 minutes, and then remove the white precipitate to obtain a transparent reaction liquid; the white precipitate is precipitated barite; the fourth step is to increase the temperature to 55-60°C and then drop a sodium hydroxide solution into the transparent reaction liquid to obtain a yellow suspension; the fifth step is to filter, wash and dry: the yellow suspension obtained in the previous step is filtered and washed with clean water, and then filtered and dried to obtain a yellow solid; the sixth step is to calcine and blast: the yellow solid is sent to a calcining furnace at 200-300°C and calcined for 20-30 minutes to obtain the obtained product.

[0005] Zinc sulfate solution has a wide range of sources and is relatively low in cost, such as zinc hydrometallurgy, rotary hearth furnace dust, and so on.

[0006] Furthermore, the mass ratio of the barium peroxide paste in the third step to the acidic zinc sulfate aqueous solution is 6% to 7%.

[0007] Furthermore, in the fourth step, sodium hydroxide solution is added dropwise until the pH value of the system is 8 to 8.5.

[0008] Furthermore, the stirring speed in the third step is 500-1000 rpm.

[0009] Furthermore, the mass concentration of the sodium hydroxide solution is 15% to 20%.

[0010] Furthermore, the fifth step drying condition is 70-80° C. for 6-8 hours.

[0011] Barium peroxide has been used in the past as bleach, mordant, disinfectant, etc.

[0012] Furthermore, the solid content of the barium peroxide paste is 85% to 90%.

[0013] Beneficial effects of the present invention: The invention discloses a production method of high-dispersion zinc oxide with a large specific surface area. The method comprises the following steps: adding barium peroxide to an acidic zinc sulfate aqueous solution for reaction, and then subjecting the mixture to sodium hydroxide solution, filter pressing, washing, drying, and calcining and blasting to obtain the high-dispersion zinc oxide with a large specific surface area. The calcining and heating action rapidly converts a yellow solid into heat energy, which can rapidly undergo self-oxidation and blasting to obtain nano zinc oxide with high purity and a large specific surface area. The method has the advantages of high yield, simple operation, low pollution, and the like. Precipitated barite powder as a byproduct can also be obtained, thereby increasing the economic benefit of the method and obtaining the characteristics of high specific surface area, surface energy, high dispersion, and the like. DETAILED DESCRIPTION

[0014] The present invention is described below with specific examples, but is not intended to be limiting of the present invention. Example 1

[0015] Raw materials and equipment: Nanhua reagent barium peroxide; Nanhua reagent ACS zinc sulfate; Jincheng reagent sodium hydroxide.

[0016] The production method of highly dispersed zinc oxide with large specific surface area comprises the following steps: The first step is to prepare a zinc sulfate aqueous solution with zinc sulfate, and adjust its pH value to 0.75 with dilute sulfuric acid to obtain a 58g / L acidic zinc sulfate aqueous solution; the second step is to premix barium peroxide with 0°C ice water to form a barium peroxide paste, and the solid content of the barium peroxide paste is 88%; the third step is to immediately stir and mix the obtained barium peroxide paste with the acidic zinc sulfate aqueous solution under 0°C ice water bath conditions for 12 minutes, with a stirring speed of 800rpm, and remove the white precipitate to obtain a transparent reaction solution; the fourth step is to increase the temperature to 58°C and then drip sodium hydroxide solution into the transparent reaction solution, drip sodium hydroxide solution until the system pH is 8.2, and the mass concentration of the sodium hydroxide solution is 18%, to obtain a yellow suspension; the fifth step is to filter, wash, and dry: the yellow suspension obtained in the previous step is filtered and washed with clean water, and then filtered and dried, and the drying condition is 75°C and dried for 7h to obtain a yellow solid; the sixth step is calcination and blasting: the yellow solid is sent to a calcining furnace at 200-300°C and calcined for 25min.

[0017] Product performance: Appearance: white powder; Zinc oxide content (calculated as dry product), ω / % ≥ 99.5; Metal content (calculated as Zn), ω / % ≤ 0.008; Hydrochloric acid insoluble matter, ω / % ≤ 0.03; Ignition loss, ω / % ≤ 0.25; Sieve residue (45μm test sieve), ω / % ≤ 0.20; Water-soluble matter, ω / % ≤ 0.15; Volatile matter at 105℃ ≤ 0.50; Lead (Pb) content ≤ 0.10; Copper (Cu) content ≤ 0.0007; Manganese (Mn) content ≤ 0.0003; Cadmium (Cd) content ≤ 0.010; Specific surface area / (㎡ / g) ≥ 70. Example 2

[0018] Raw materials and equipment: Hejiang Huanan Inorganic Salt Barium Peroxide; Nanjing University Optoelectronic Materials Zinc Sulfate; Hong Sifang Sodium Hydroxide.

[0019] The production method of highly dispersed zinc oxide with large specific surface area comprises the following steps: The first step is to prepare a zinc sulfate aqueous solution with zinc sulfate, and adjust its pH value to 0.5 with dilute sulfuric acid to obtain a 55g / L acidic zinc sulfate aqueous solution; the second step is to premix barium peroxide with 0°C ice water to form a barium peroxide paste, and the solid content of the barium peroxide paste is 85%; the third step is to immediately stir and mix the obtained barium peroxide paste with the acidic zinc sulfate aqueous solution in a 0°C ice water bath for 10 minutes at a stirring speed of 500rpm, and remove the white precipitate to obtain a transparent reaction solution; the fourth step is to increase the temperature to 55-60°C and then drip sodium hydroxide solution into the transparent reaction solution, drip sodium hydroxide solution until the system pH is 8, and the mass concentration of the sodium hydroxide solution is 15%, and a yellow suspension is obtained; the fifth step is to filter, wash, and dry: the yellow suspension obtained in the previous step is filtered and washed with clean water, and then filtered and dried, and the drying condition is 70°C and dried for 6h to obtain a yellow solid; the sixth step is calcination and blasting: the yellow solid is sent to a 200°C calcining furnace and calcined for 30 minutes.

[0020] Product performance: Appearance: white powder; Zinc oxide content (calculated as dry product), ω / % ≥ 99.5; Metal content (calculated as Zn), ω / % ≤ 0.008; Hydrochloric acid insoluble matter, ω / % ≤ 0.03; Ignition loss, ω / % ≤ 0.25; Sieve residue (45μm test sieve), ω / % ≤ 0.20; Water-soluble matter, ω / % ≤ 0.15; Volatile matter at 105℃ ≤ 0.50; Lead (Pb) content ≤ 0.10; Copper (Cu) content ≤ 0.0007; Manganese (Mn) content ≤ 0.0003; Cadmium (Cd) content ≤ 0.010; Specific surface area / (㎡ / g) ≥ 68. Example 3

[0021] Raw materials and equipment: barium peroxide from Guanghua Technology; zinc sulfate from Feidong Zhengfan; sodium hydroxide from Ruixiang Chemical.

[0022] The production method of highly dispersed zinc oxide with large specific surface area comprises the following steps: The first step is to prepare a zinc sulfate aqueous solution with zinc sulfate, and adjust its pH value to 1 with dilute sulfuric acid to obtain a 60g / L acidic zinc sulfate aqueous solution; the second step is to premix barium peroxide with 0°C ice water to form a barium peroxide paste, and the solid content of the barium peroxide paste is 85% to 90%; the third step is to immediately stir and mix the obtained barium peroxide paste with the acidic zinc sulfate aqueous solution under 0°C ice water bath conditions for 15 minutes, with a stirring speed of 1000rpm, and remove the white precipitate to obtain a transparent reaction solution; the fourth step is to increase the temperature to 60°C and then drip sodium hydroxide solution into the transparent reaction solution, drip sodium hydroxide solution until the system pH is 8.5, and the mass concentration of the sodium hydroxide solution is 20%, to obtain a yellow suspension; the fifth step is to filter, wash, and dry: the yellow suspension obtained in the previous step is filtered and washed with clean water, and then filtered and dried, and the drying condition is 80°C and dried for 8h to obtain a yellow solid; the sixth step is calcination and blasting: the yellow solid is sent to a 300°C calcining furnace and calcined for 20 minutes.

[0023] Product performance: Appearance: white powder; Zinc oxide content (calculated as dry product), ω / % ≥ 99.5; Metal content (calculated as Zn), ω / % ≤ 0.008; Hydrochloric acid insoluble matter, ω / % ≤ 0.03; Ignition loss, ω / % ≤ 0.25; Sieve residue (45μm test sieve), ω / % ≤ 0.20; Water-soluble matter, ω / % ≤ 0.15; Volatile matter at 105℃ ≤ 0.50; Lead (Pb) content ≤ 0.10; Copper (Cu) content ≤ 0.0007; Manganese (Mn) content ≤ 0.0003; Cadmium (Cd) content ≤ 0.010; Specific surface area / (㎡ / g) ≥ 80.

[0024] Note: The determination of sieve residue shall be carried out in accordance with the provisions of GB / T5211.18-2015, and the sample shall be 10g. The determination of water-soluble matter shall be carried out in accordance with the provisions of GB / T5211.2-2003, and the sample shall be 10g. The determination of volatile matter at 105℃ shall be carried out in accordance with the provisions of GB / T5211.3-2020, and the sample shall be 5g. Determination method of lead (Pb) content Instrument conditions Instrument conditions are as follows: - Light source: lead hollow cathode lamp; - Wavelength: 283.3nm; - Flame: acetylene-air. Determination method Weigh 5g sample, moisten with a small amount of water, add hydrochloric acid solution (20%) until the sample is dissolved, and dilute to 250mL. Take 25mL, a total of four portions. Determine according to the provisions of 7.2.2 of GB / T9723-2007, and the results are calculated according to the provisions of 7.2.3 of GB / T9723-2007. Copper (Cu) content determination method Instrument conditions Instrument conditions are as follows: - Light source: copper hollow cathode lamp; - Wavelength: 324.7nm; - Flame: acetylene-air. Determination method Weigh 5g sample, moisten with a small amount of water, add hydrochloric acid solution (20%) until the sample is dissolved, and dilute to 250mL. Take 25mL, a total of four portions. Determine according to the provisions of 7.2.2 of GB / T9723-2007, and the results are calculated according to the provisions of 7.2.3 of GB / T9723-2007. Manganese (Mn) content determination method Instrument conditions Instrument conditions are as follows: - Light source: manganese hollow cathode lamp; - Wavelength: 279.5nm; - Flame: acetylene-air. Determination method Weigh 5g sample, moisten with a small amount of water, add hydrochloric acid solution (20%) until the sample is dissolved, and dilute to 250mL. Take 25mL, a total of four portions. Determine according to the provisions of 7.2.2 of GB / T9723-2007, and calculate the results according to the provisions of 7.2.3 of GB / T9723-2007. Determination method of cadmium (Cd) content Instrument conditions Instrument conditions are as follows: - Light source: cadmium hollow cathode lamp; - Wavelength: 228.8nm; - Flame: acetylene-air. Determination method Weigh 5g sample, moisten with a small amount of water, add hydrochloric acid solution (20%) until the sample dissolves, and dilute to 250mL. Take 25mL, a total of four portions. Determine according to the provisions of 7.2.2 of GB / T9723-2007, and calculate the results according to the provisions of 7.2.3 of GB / T9723-2007. Determination method of iron (Fe) content - Instrument conditions Instrument conditions are as follows: - Light source: iron hollow cathode lamp; - Wavelength: 248.3nm; - Flame: acetylene-air. Determination method Weigh 5g sample, moisten with a small amount of water, add hydrochloric acid solution (20%) until the sample dissolves, and dilute to 250mL. Take 25mL, a total of four portions. Determine according to the provisions of 7.2.2 of GB / T9723-2007, and calculate the results according to the provisions of 7.2.3 of GB / T9723-2007. Determination method Weigh 0.5g sample, accurate to 0.0001g.Place the sample in a 250ml beaker, add 30ml nitric acid (1+1), heat and dissolve completely, remove and cool, transfer to a 100ml volumetric flask, dilute to scale with nitric acid (1+1), and mix well. Determine according to the provisions of 6.3 in GB / T12689.12-2004, and calculate the results according to the provisions of Chapter 7 in GB / T12689.12-2004. Determination of specific surface area Weigh an appropriate amount of sample to an accuracy of 0.0002g, place it in a sample tube, degas at 70℃ for 4h, place it on a specific surface area meter, and determine it according to the provisions of GB / T19587-2017. The results are calculated according to the BET equation. The oil absorption is carried out according to the provisions of GB / T5211.15-2014, and the sample weight is 10g. The color is carried out according to the provisions of GB / T1864-2012. The tinting power shall be in accordance with the provisions of GB / T5211.16-2007. The zinc oxide content, ignition loss, metal content and hydrochloric acid insoluble matter shall refer to GB / T3185-2016.

Claims

1. A method for producing highly dispersed zinc oxide with a large specific surface area, characterized in that: The following steps are involved: The first step is to prepare a zinc sulfate aqueous solution by taking zinc sulfate, and adjusting its pH value to 0.5-1 with dilute sulfuric acid to obtain a 55-60 g / L acidic zinc sulfate aqueous solution; the second step is to premix barium peroxide with 0° C. ice water to form a barium peroxide paste; The third step is to immediately mix the obtained barium peroxide paste with an acidic zinc sulfate aqueous solution in an ice-water bath at 0°C for 10 to 15 minutes, remove the white precipitate, and obtain a transparent reaction solution; the fourth step is to increase the temperature to 55 to 60°C and then drop a sodium hydroxide solution into the transparent reaction solution to obtain a yellow suspension; the fifth step is to filter, wash, and dry: the yellow suspension obtained in the previous step is filtered, washed with clean water, and then filtered and dried to obtain a yellow solid; the sixth step is to calcine and blast: the yellow solid is sent to a calcining furnace at 200 to 300°C and calcined for 20 to 30 minutes to obtain the obtained product.

2. The method for producing highly dispersed zinc oxide with a large specific surface area according to claim 1, characterized in that: The mass ratio of the barium peroxide paste in the third step to the acidic zinc sulfate aqueous solution is 6% to 7%.

3. The method for producing highly dispersed zinc oxide with large specific surface area according to claim 1, characterized in that: In the fourth step, sodium hydroxide solution is added dropwise until the pH value of the system is 8 to 8.

5.

4. The method for producing highly dispersed zinc oxide with a large specific surface area according to claim 1, characterized in that: The third step is stirring at a speed of 500-1000 rpm.

5. The method for producing highly dispersed zinc oxide with large specific surface area according to claim 1, characterized in that: The mass concentration of the sodium hydroxide solution is 15% to 20%.

6. The method for producing highly dispersed zinc oxide with a large specific surface area according to claim 1, characterized in that: The fifth step drying condition is 70-80° C. for 6-8 hours.

7. The method for producing highly dispersed zinc oxide with a large specific surface area according to claim 1, characterized in that: The solid content of the barium peroxide paste is 85% to 90%.

Citation Information

Patent Citations

  • Preparation method of ZnO with large specific surface area

    CN109704388A

  • Method for producing nano zinc peroxide and zinc oxide by using solar

    CN101152957A

  • Preparation method for nanometer zinc oxide

    CN101214993A

  • Rounded zinc peroxide particles, rounded zinc oxide particles, manufacturing method therefor, cosmetic material, and heat-dissipating filler

    CN103502142A

  • Zinc oxide and production method of zinc oxide as well as cosmetic, resin composition, coating composition, and inorganic powder using zinc oxide

    JP2014221708A