Preparation method of CuGa2O4 nanowire

Through optimizing reaction conditions and chemical vapor deposition method without metal catalysts, high-efficiency and low-cost CuGa2O4 nanowires were successfully prepared, which solved the problems of difficult and cost in the existing technology, and achieved high purity and excellent performance of nanowires .

CN118877927APending Publication Date: 2024-11-01LIAONING NORMAL UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410936482.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The preparation method of CuGa2O4 nanowires in the prior art relies on precious metal catalysts, which increases complexity and cost, and requires long-term reaction conditions at high temperatures, resulting in high production difficulty and cost, and research is still insufficient.

Method used

By optimizing the reaction conditions, using a chemical vapor deposition method without metal catalyst, using copper oxide powder and gallium oxide powder to mix in a certain proportion, and adding carbon powder, place it in a corundum boat for nanowire growth at high temperature, using inert carrier gas And control the oxygen flow rate and time, reduce the reaction temperature to below 1100°C, and shorten the growth time.

Benefits of technology

The preparation of CuGa2O4 nanowires without metal catalysts is realized, which simplifies the process, avoids impurity problems, reduces production costs, improves the purity and performance of nanowires, and significantly reduces energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118877927A_ABST
    Figure CN118877927A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a CuGa2O4 nanowire, which comprises the following steps: mixing copper oxide powder and gallium oxide powder according to a mass ratio of 1: 1-4: 1, adding carbon powder which is 1-2 times of the mass of the mixture, uniformly mixing to obtain a reaction source material, placing the reaction source material in a corundum boat, placing a clean substrate on the corundum boat, keeping the distance between the substrate and the reaction source material at 1-2cm, and carrying out heat treatment on the substrate to obtain the CuGa2O4 nanowire. Then pushing the corundum boat into a high-temperature heating area in a quartz tube of chemical vapor deposition equipment, setting the reaction temperature for nanowire growth to be 1000-1100 DEG C, introducing inert carrier gas into the quartz tube, controlling the flow of the carrier gas to be 80-180mL / min, introducing oxygen when the heating temperature reaches the reaction temperature, continuing for 20-40 minutes, controlling the flow of the oxygen to be 10-30mL / min, closing the oxygen, keeping the flow of the inert carrier gas, and keeping the flow of the inert carrier gas to be 10-30mL / min; and after cooling, taking out a sample to obtain a CuGa2O4 nanowire product. The invention provides an efficient and economical preparation method of the CuGa2O4 nanowire, and low-cost and high-quality preparation of the CuGa2O4 nanowire is realized by optimizing reaction conditions under the condition of not using a metal catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nanomaterials, and in particular to a method for preparing CuGa2O4 nanowires. Background Art

[0002] CuGa2O4 is a spinel oxide semiconductor material with a unique cubic crystal structure and face-centered cubic lattice (space group The lattice constant is ) endows it with excellent physical and chemical properties, especially in the fields of gas sensing, catalytic hydrogen production and microwave dielectrics, showing significant application potential. In addition, CuGa2O4, due to its high transmittance and wide bandgap (about 2.5-4.4eV), indicates a wide range of application prospects in the fields of high-performance solar-blind detectors and new optoelectronic devices. As a one-dimensional nanomaterial, nanowires have excellent performance in specific surface area, crystal quality, mechanical toughness, gas sensitivity and optoelectronic properties, and are of great scientific research and application value. However, the current research on CuGa2O4 materials is still insufficient, especially the research on its nanowire morphology is almost blank.

[0003] In the prior art, the preparation of gallium-containing oxide nanowires by chemical vapor deposition (CVD) often relies on precious metal catalysts such as platinum and gold, which not only increases the complexity and cost of preparation, but also may introduce impurities that affect material properties. Although the patent with application number 201811035848.2 proposes a technical solution for preparing gallium-containing oxide nanowires by CVD technology without catalyst, it requires extremely high reaction temperature (above 1100°C), long growth time (more than 1 hour) and large amounts of oxygen and carrier gas, which significantly increases the difficulty and cost of preparation. Summary of the invention

[0004] In view of the technical problems existing in the prior art, the present invention aims to provide a more efficient and economical method for preparing CuGa2O4 nanowires, which can achieve low-cost and high-quality preparation of CuGa2O4 nanowires by optimizing the reaction conditions and without using metal catalysts.

[0005] A method for preparing CuGa2O4 nanowires, characterized in that it comprises the following steps:

[0006] S1: mixing copper oxide powder and gallium oxide powder in a mass ratio of 1:1 to 4:1, adding carbon powder to the mixture and mixing evenly to obtain a reaction source material, wherein the amount of the carbon powder added is 1 to 2 times the mass of the mixture;

[0007] S2: placing the reaction source material in a corundum boat, placing a clean substrate on the corundum boat, the substrate being 1 to 2 cm away from the reaction source material, and then pushing the corundum boat into a high-temperature heating zone in a quartz tube of a chemical vapor deposition device, setting the reaction temperature for nanowire growth to 1000 to 1100° C.;

[0008] S3: introducing an inert carrier gas into the quartz tube, wherein the flow rate of the inert carrier gas is 80 to 180 mL / min;

[0009] S4: When the heating temperature reaches the reaction temperature, oxygen is introduced for 20 to 40 minutes, and the oxygen flow rate is 10 to 30 mL / min;

[0010] S5: After turning off the oxygen, maintain the inert carrier gas flow rate, and take out the sample after cooling down to obtain the CuGa2O4 nanowire product.

[0011] Furthermore, the copper oxide powder has a purity greater than 99%.

[0012] Furthermore, the substrate is made of sapphire or silicon.

[0013] Furthermore, the inert carrier gas is argon.

[0014] In summary, the present invention has the following beneficial effects:

[0015] First, the present invention realizes the direct preparation of CuGa2O4 nanowires without any metal catalyst, which not only simplifies the preparation process, avoids the problem of impurities that may be introduced by the catalyst, ensures the high purity and excellent performance of the nanowires, but also significantly reduces the production cost.

[0016] Second, the present invention reduces the reaction temperature to below 1100°C and significantly shortens the growth time of nanowires to less than 40 minutes, reducing energy consumption. At the same time, by precisely controlling the ventilation volume and ventilation time of oxygen and carrier gas, the preparation cost is further reduced. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0018] Figure 1 This is a scanning electron microscope photograph of the sample obtained in Example 1 of the present invention.

[0019] Figure 2It is the X-ray diffraction spectrum of the sample obtained in Example 1 of the present invention.

[0020] Figure 3 This is a scanning electron microscope photograph of the sample obtained in Example 2 of the present invention.

[0021] Figure 4 This is a scanning electron microscope photograph of the sample obtained in Example 3 of the present invention. DETAILED DESCRIPTION

[0022] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0023] A method for preparing CuGa2O4 nanowires, characterized in that it comprises the following steps:

[0024] S1: mixing copper oxide powder and gallium oxide powder in a mass ratio of 1:1 to 4:1, adding carbon powder to the mixture and mixing evenly to obtain a reaction source material, wherein the amount of the carbon powder added is 1 to 2 times the mass of the mixture;

[0025] S2: placing the reaction source material in a corundum boat, placing a clean substrate on the corundum boat, the substrate being 1 to 2 cm away from the reaction source material, and then pushing the corundum boat into a high-temperature heating zone in a quartz tube of a chemical vapor deposition device, setting the reaction temperature for nanowire growth to 1000 to 1100° C.;

[0026] S3: introducing an inert carrier gas into the quartz tube, wherein the flow rate of the inert carrier gas is 80 to 180 mL / min;

[0027] S4: When the heating temperature reaches the reaction temperature, oxygen is introduced for 20 to 40 minutes, and the oxygen flow rate is 10 to 30 mL / min;

[0028] S5: After turning off the oxygen, maintain the inert carrier gas flow rate, and take out the sample after cooling down to obtain the CuGa2O4 nanowire product.

[0029] This scheme realizes the direct preparation of CuGa2O4 nanowires without any metal catalyst. It not only simplifies the preparation process, avoids the problem of impurities that may be introduced by the catalyst, ensures the high purity and excellent performance of the nanowires, but also significantly reduces the production cost. It reduces the reaction temperature to below 1100°C and greatly shortens the growth time of the nanowires to less than 40 minutes, reducing energy consumption. At the same time, by precisely controlling the ventilation volume and ventilation time of oxygen and carrier gas, the preparation cost is further reduced.

[0030] Furthermore, the copper oxide powder has a purity greater than 99%.

[0031] In this scheme, high-purity copper oxide powder is used to reduce the impact of impurities on the crystallinity and structural integrity of the nanowires during growth. In addition, high-purity copper oxide powder has higher reactivity, which helps to obtain better growth effects and more uniform nanowire diameters. The prepared nanowires have better stability and higher purity, avoiding electron scattering and phonon scattering caused by impurities.

[0032] Furthermore, the substrate is made of sapphire or silicon.

[0033] In this scheme, CuGa2O4 nanowires prepared on sapphire or silicon substrates are selected, with a diameter distribution of 50 to 80 nm, a length of about 10 to 20 μm, and uniform size. Nanowires, due to their large specific surface area, help to achieve more efficient light absorption and conversion in optoelectronic devices, and improve the photoelectric conversion efficiency of the device. In addition, they have a shorter electron transmission path and less electron scattering, thereby improving the transmission efficiency of electrons in nanowires. This is of great significance for the preparation of high-speed electronic and optoelectronic devices.

[0034] Furthermore, the inert carrier gas is argon.

[0035] The preferred argon gas in this scheme has significant advantages such as low thermal enthalpy and excellent inertness. It improves energy utilization and ensures process stability during the preparation of nanowires, and the prepared nanowire products have high purity and quality.

[0036] Example 1

[0037] The preparation of CuGa2O4 nanowires is carried out according to the following steps:

[0038] (1) Copper oxide powder and gallium oxide powder with a purity greater than 99% are mixed in a mass ratio of 1:1, and carbon powder is selected as a reducing agent, the mass of which is 1.5 times the total mass of the copper oxide powder and the gallium oxide powder. The three are mixed to form a reaction source material, and the reaction source is placed in a corundum boat, and a cleaned sapphire substrate is inverted on the corundum boat directly above the reaction source, 1.5 cm away from the reaction source, and then the corundum boat is pushed into the high-temperature heating zone in the quartz tube of the chemical vapor deposition equipment;

[0039] (2) introducing argon gas as carrier gas into the quartz tube at a flow rate of 180 mL / min;

[0040] (3) When the heating temperature reaches 1050°C, oxygen is introduced at a flow rate of 10 mL / min and the growth time is 30 minutes;

[0041] (4) After the growth is completed, turn off the oxygen, maintain the argon flow, and wait until the temperature drops to room temperature before taking out the sample.

[0042] Example 2

[0043] The preparation of CuGa2O4 nanowires is carried out according to the following steps:

[0044] (1) Copper oxide powder and gallium oxide powder with a purity greater than 99% are mixed in a mass ratio of 4:1, and carbon powder is selected as a reducing agent, the mass of which is the same as the sum of the copper oxide powder and the gallium oxide powder. The three are mixed to form a reaction source material, and the reaction source is placed in a corundum boat, and a cleaned sapphire substrate is inverted on the corundum boat directly above the reaction source, 1.5 cm away from the reaction source, and then the corundum boat is pushed into the high-temperature heating zone in the quartz tube of the chemical vapor deposition equipment;

[0045] (2) introducing argon gas as carrier gas into the quartz tube at a flow rate of 80 mL / min;

[0046] (3) When the heating temperature reaches 1000°C, oxygen is introduced at a flow rate of 20 mL / min and the growth time is 40 minutes;

[0047] (4) After the growth is completed, turn off the oxygen, maintain the argon flow, and wait until the temperature drops to room temperature before taking out the sample.

[0048] Example 3

[0049] The preparation of CuGa2O4 nanowires is carried out according to the following steps:

[0050] (1) Copper oxide powder and gallium oxide powder with a purity greater than 99% are mixed in a mass ratio of 1:1, and carbon powder is selected as a reducing agent, whose mass is twice the total of the copper oxide powder and the gallium oxide powder. The three are mixed to form a reaction source material, and the reaction source is placed in a corundum boat, and a cleaned silicon substrate is inverted on the corundum boat directly above the reaction source, 1.5 cm away from the reaction source, and then the corundum boat is pushed into the high-temperature heating zone in the quartz tube of the chemical vapor deposition equipment;

[0051] (2) introducing argon gas as carrier gas into the quartz tube at a flow rate of 120 mL / min;

[0052] (3) When the heating temperature reaches 1100°C, oxygen is introduced at a flow rate of 30 mL / min and the growth time is 20 minutes;

[0053] (4) After the growth is completed, turn off the oxygen, maintain the argon flow, and wait until the temperature drops to room temperature before taking out the sample.

[0054] Example 4

[0055] The preparation of CuGa2O4 nanowires is carried out according to the following steps:

[0056] (1) Copper oxide powder and gallium oxide powder with a purity greater than 99% are mixed in a mass ratio of 2.5:1, and carbon powder is selected as a reducing agent, the mass of which is 1.5 times the total of the copper oxide powder and the gallium oxide powder. The three are mixed to form a reaction source material, and the reaction source is placed in a corundum boat, and a cleaned silicon substrate is inverted on the corundum boat directly above the reaction source, 1.5 cm away from the reaction source, and then the corundum boat is pushed into the high-temperature heating zone in the quartz tube of the chemical vapor deposition equipment;

[0057] (2) introducing argon gas as carrier gas into the quartz tube at a flow rate of 150 mL / min;

[0058] (3) When the heating temperature reaches 1050°C, oxygen is introduced at a flow rate of 10 mL / min and the growth time is 30 minutes;

[0059] (4) After the growth is completed, turn off the oxygen, maintain the argon flow, and wait until the temperature drops to room temperature before taking out the sample.

[0060] The specific experimental conditions of each embodiment are shown in Table 1:

[0061] Table 1 List of experimental conditions corresponding to each embodiment

[0062]

[0063] Test results and analysis

[0064] The present invention implements and strictly verifies the technical solutions proposed in Examples 1 to 3 in detail. The performance indicators of the CuGa2O4 nanowire samples prepared in each example are shown in Table 2:

[0065] Table 2 Performance indicators of nanowire samples prepared in Example

[0066] sample Nanowire morphology Nanowire diameter / nm Nanowire length / μm Example 1 High density, uniform size Approx. 50 Approx. 20 Example 2 High density, uniform size Approx. 80 Approx. 10 Example 3 High density, uniform size Approx. 50 Approx. 20

[0067] Scanning electron microscope (SEM) image of the CuGa2O4 nanowire sample prepared in Example 1 ( Figure 1 ) clearly showed a large area of ​​uniformly distributed nanowire arrays on the sample surface. The diameter and length of these nanowires were controlled at about 50nm and 20μm, showing good morphological consistency. Further X-ray diffraction (XRD) analysis ( Figure 2 ), except for the characteristic peak originating from the (006) crystal plane of the sapphire substrate located at 41.7°, all other diffraction peaks accurately match the standard card of CuGa2O4 (JCPDS 44-0183), confirming that the chemical composition of the prepared nanowires is CuGa2O4.

[0068] In Example 2, the mass ratio of copper oxide powder to gallium oxide powder was adjusted from 1:1 to 4:1. The SEM image ( Figure 3 ) revealed a significant change in the morphology of the prepared CuGa2O4 nanowires. Specifically, the diameter of the nanowires increased to about 80nm, while the length was shortened to about 10μm. This change shows that the adjustment of the raw material ratio can directly affect the growth dynamics of the nanowires, thereby controlling their size characteristics, providing an effective means for the customized synthesis of nanomaterials.

[0069] Example 3 further explores the effect of different substrate materials on the growth of CuGa2O4 nanowires. SEM image ( Figure 4 ) showed that the nanowires grown on the silicon substrate also exhibited the characteristics of high density and uniform distribution, and their morphology was highly similar to that of the nanowires grown on the sapphire substrate, verifying the wide applicability of the preparation method and the flexibility of the substrate material.

[0070] In summary, this scheme successfully achieved low-cost and high-efficiency preparation of CuGa2O4 nanowires based on optimized preparation conditions. By lowering the reaction temperature to below 1100°C and significantly shortening the growth time to within 40 minutes, not only the energy consumption was effectively reduced, but also the preparation cost was further reduced by finely controlling the ventilation volume and time of oxygen and carrier gas. More importantly, the entire preparation process does not rely on any metal catalysts, which not only simplifies the process flow, avoids potential impurity problems introduced by catalysts, ensures the high purity and excellent performance of the nanowires, but also significantly reduces production costs.

[0071] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing CuGa2O4 nanowires, characterized in that: The following steps are involved: S1: mixing copper oxide powder and gallium oxide powder in a mass ratio of 1:1 to 4:1, adding carbon powder to the mixture and mixing evenly to obtain a reaction source material, wherein the amount of the carbon powder added is 1 to 2 times the mass of the mixture; S2: placing the reaction source material in a corundum boat, placing a clean substrate on the corundum boat, the substrate being 1 to 2 cm away from the reaction source material, and then pushing the corundum boat into a high-temperature heating zone in a quartz tube of a chemical vapor deposition device, setting the reaction temperature for nanowire growth to 1000 to 1100° C.; S3: introducing an inert carrier gas into the quartz tube, wherein the flow rate of the inert carrier gas is 80 to 180 mL / min; S4: When the heating temperature reaches the reaction temperature, oxygen is introduced for 20 to 40 minutes, and the oxygen flow rate is 10 to 30 mL / min; S5: After turning off the oxygen, maintain the inert carrier gas flow rate, and take out the sample after cooling down to obtain the CuGa2O4 nanowire product.

2. The method for preparing CuGa2O4 nanowires according to claim 1, characterized in that: The copper oxide powder has a purity greater than 99%.

3. The method for preparing CuGa2O4 nanowires according to claim 1, characterized in that: The substrate is made of sapphire or silicon.

4. The method for preparing CuGa2O4 nanowires according to claim 1, characterized in that: The inert carrier gas is argon.