Preparation process of hollow TiO2 powder

Through the hydrothermal reaction and etching process of tetrabutyl titanate and polyethylene glycol, the problems of incomplete structure and complex template removal in the preparation of hollow TiO2 powder were solved, and hollow TiO2 powder with high specific surface area and excellent photocatalytic properties were obtained. .

CN118877933AInactive Publication Date: 2024-11-01SHAANXI AEROSPACE INTELLIGENT MANUFACTURING NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411145043.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the existing hollow TiO2 powder preparation process, it is difficult to accurately control the integrity of the hollow structure, and the template removal process is complex and costly, resulting in unsatisfactory specific surface area and photocatalytic activity.

Method used

Using tetrabutyl titanate as the titanium source and polyethylene glycol as the template agent, the TiO2 precursor is formed through hydrothermal reaction and etching steps, followed by template removal using acetone, control reaction temperature and time, and optimize etching conditions to obtain high ratio Hollow TiO2 powder with surface area and excellent photocatalytic properties.

Benefits of technology

It realizes precise control of hollow structures, improves specific surface area and photocatalytic performance, and is suitable for a variety of application fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention discloses a preparation process of hollow T O2 powder, and relates to the technical field of chemical materials, the hollow T O2 powder comprises a titanium source serving as an initial raw material and a surfactant serving as a template agent, and the preparation process comprises the following steps: dissolving the template agent in a solvent, uniformly stirring to form a template solution, dissolving or dispersing the titanium source in the template solution, and preparing a hollow T O2 powder solution; the preparation method comprises the following steps: adding a titanium source and a template into a hydrothermal reaction kettle to form a uniform titanium source-template mixed solution, putting the titanium source-template mixed solution into the hydrothermal reaction kettle, sealing, putting into a drying oven, reacting for 6 hours at 150 DEG C to form a Ti O2 precursor, and putting the Ti O2 precursor into an extracting solvent to remove the template to obtain hollow Ti O2 powder. The uniform and complete hollow structure can be more effectively formed by accurately controlling the concentration of the template agent, the hydrothermal reaction temperature, the hydrothermal reaction time and other parameters; by optimizing etching conditions and time, the integrity of the hollow structure can be kept while the template is removed; the hollow Ti O2 powder with higher specific surface area and better photocatalytic performance can be prepared, and is suitable for more fields.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of chemical materials, in particular to a preparation process of hollow TiO2 powder. Background Art

[0002] Titanium dioxide (chemical formula: TiO2), a white solid or powdered amphoteric oxide, is the best white pigment, commonly known as titanium white. Titanium white has strong adhesion, is not easy to undergo chemical changes, and is always snow-white. What is particularly valuable is that titanium white is non-toxic and has a high melting point. It is used to make refractory glass, glaze, enamel, clay, high-temperature resistant laboratory equipment, etc. There are three types of titanium dioxide crystals in nature, anatase, rutile and brookite. Rutile TiO2 is the most stable crystal structure with fewer defects in the lattice. Titanium dioxide can be extracted from rutile by acid decomposition, or obtained by decomposition of titanium tetrachloride. Titanium dioxide is stable in nature and is widely used as a white pigment in paint. It has good hiding power, similar to lead white, but unlike lead white, it will not turn black; it has the same durability as zinc white. Titanium dioxide is also used as a matting agent for enamel, which can produce a very bright, hard and acid-resistant enamel glaze finish.

[0003] In the prior art, the preparation process of hollow TiO2 powder has the following shortcomings:

[0004] 1. The formation of hollow structures is often difficult to accurately control, resulting in incomplete hollow structures or serious agglomeration.

[0005] 2. Template removal usually requires the use of stronger chemical etchants or high-temperature treatment, which not only increases the complexity and cost of preparation, but may also damage the hollow structure.

[0006] 3. The prepared hollow TiO2 powder may not be ideal in terms of specific surface area, photocatalytic activity, etc.

[0007] In view of this, the present invention is proposed. Summary of the invention

[0008] The purpose of the present application is to provide a process for preparing hollow TiO2 powder, comprising a titanium source as a starting material and a surfactant as a template;

[0009] The preparation process comprises the following steps:

[0010] Step 1: dissolve the template in a solvent and stir evenly to form a template solution;

[0011] Step 2: dissolving or dispersing the titanium source in the template solution to form a uniform titanium source-template mixed solution;

[0012] Step 3: Place the titanium source-template mixed solution into a hydrothermal reactor, seal it, and place it in an oven to react at 150°C for 6 hours to form a TiO2 precursor;

[0013] Step 4: Place the TiO2 precursor in an extraction solvent to remove the template and obtain hollow TiO2 powder;

[0014] Step 5: Wash, dry and grind the obtained hollow TiO2 powder.

[0015] Furthermore, the template agent is polyethylene glycol with a concentration of 0.1M.

[0016] Furthermore, the solvent is ethanol and water in a volume ratio of 1:1, and the stirring time in step 1 is 30 minutes and the stirring speed is 500 rpm.

[0017] Furthermore, the titanium source is 0.01-0.05M tetrabutyl titanate, and the volume ratio of the titanium source to the template solution is 1:10.

[0018] Furthermore, the extraction solvent is acetone. When the TiO2 precursor is placed in acetone to remove the template, the mixture of the TiO2 precursor and acetone is stirred for 30 minutes.

[0019] Furthermore, in step 3, when adjusting the pH, aqueous ammonia is used as a regulator to control the pH of the reaction.

[0020] Furthermore, in step 3, the titanium source is stirred during the reaction, and the color gradually changes from transparent to milky white during the stirring process.

[0021] Furthermore, in step 4, the volume ratio of the extraction solvent to the TiO2 precursor is 1:1.

[0022] Further, in step 5, the hollow TiO2 powder is ground so that the particle size of the hollow TiO2 powder is 50 nm.

[0023] Furthermore, in step 5, the hollow TiO2 powder is washed and diluted with deionized water.

[0024] By adopting the above technical solution, the present invention has the following beneficial effects:

[0025] 1. By precisely controlling parameters such as template concentration, hydrothermal reaction temperature and time, a uniform and complete hollow structure can be formed more effectively.

[0026] 2. By optimizing etching conditions and time, the integrity of the hollow structure can be maintained while removing the template.

[0027] 3. Hollow TiO2 powder with higher specific surface area and better photocatalytic performance can be prepared, which is suitable for more fields.

[0028] The specific embodiments of the present invention are described in further detail. DETAILED DESCRIPTION

[0029] The present application embodiment provides a process for preparing hollow TiO2 powder, using a titanium source as a starting material and a surfactant as a template;

[0030] The preparation process comprises the following steps:

[0031] Step 1: dissolve the template in a solvent and stir evenly to form a template solution;

[0032] Step 2: dissolving or dispersing the titanium source in the template solution to form a uniform titanium source-template mixed solution;

[0033] Step 3: Place the titanium source-template mixed solution into a hydrothermal reactor, seal it and place it in an oven to react at 150°C for 6 hours to allow the titanium source to undergo hydrolysis and polycondensation reactions on the template surface to form a TiO2 precursor;

[0034] Step 4: Place the TiO2 precursor in an extraction solvent to remove the template and obtain a hollow TiO2 powder. Specifically, cool the TiO2 precursor to room temperature and add it to a 0.5M NaOH solution, etch it at 90°C for 6 hours to remove the template, and collect the etched product by centrifugation to ensure that the template is completely removed;

[0035] Step 5: Wash, dry and grind the obtained hollow TiO2 powder. When drying the hollow TiO2 powder, put it into an oven and dry it at 80°C for 12 hours. After drying, the hollow TiO2 powder is obtained by mechanical grinding.

[0036] The template agent was polyethylene glycol at a concentration of 0.1 M.

[0037] The solvent is ethanol and water in a volume ratio of 1:1, and the stirring time in step 1 is 30 min and the stirring speed is 500 rpm.

[0038] The titanium source is 0.01-0.05M tetrabutyl titanate, and the volume ratio of the titanium source to the template solution is 1:10.

[0039] The extraction solvent is acetone. When the TiO2 precursor is placed in acetone to remove the template, the mixed solution of the TiO2 precursor and acetone is stirred for 30 minutes.

[0040] In step 3, when adjusting the pH, ammonia water is used as a regulator to control the pH of the reaction.

[0041] In step 3, the titanium source is stirred during the reaction, and the color gradually changes from transparent to milky white during the stirring process.

[0042] In step 4, the volume ratio of the extraction solvent to the TiO2 precursor is 1:1.

[0043] In step 5, the hollow TiO2 powder is ground so that the particle size of the hollow TiO2 powder is 50 nm.

[0044] In step 5, the hollow TiO2 powder is washed and diluted with deionized water.

[0045] The specific surface area was measured by BET method and was about 180 m 2 / g, through TEM observation, obvious hollow structure and clear shell layer can be seen, and under simulated sunlight, the photocatalytic degradation efficiency can reach more than 95%.

[0046] Comparative Example (Standard Conditions)

[0047] Weigh a certain amount of polyethylene glycol and dissolve it in ethanol to prepare a 0.1M polyethylene glycol solution. Stir it at room temperature for 30 minutes to ensure that the polyethylene glycol is completely dissolved. Slowly add tetrabutyl titanate to the polyethylene glycol solution, keep the stirring speed at 500rpm, and continue stirring for 30 minutes to fully mix the titanium source and the template. Transfer the mixed solution to a hydrothermal reactor, seal it and place it in an oven to react at 150°C for 6 hours. Pay attention to monitoring the temperature and pressure during the reaction. After the reaction is completed, take out the product and cool it to room temperature. Add the product to a 0.5M NaOH solution and etch it at 90°C for 6 hours. After etching, collect the product by centrifugation and wash it alternately with deionized water and ethanol several times. Place the washed product in an oven and dry it at 80°C for 12 hours. The dried product is mechanically ground to obtain hollow TiO2 powder. The results are as follows: The prepared hollow TiO2 powder has a complete hollow structure with a specific surface area of ​​about 180m 2 / g, with excellent photocatalytic performance.

[0048] Example 1 (Reducing the template concentration)

[0049] Weigh a certain amount of polyethylene glycol and dissolve it in ethanol to prepare a 0.05M polyethylene glycol solution. Stir it at room temperature for 30 minutes to ensure that the polyethylene glycol is completely dissolved. Slowly add tetrabutyl titanate to the polyethylene glycol solution, keep the stirring speed at 500rpm, and continue stirring for 30 minutes to fully mix the titanium source and the template. Transfer the mixed solution to a hydrothermal reactor, seal it and place it in an oven to react at 150℃ for 6 hours. Pay attention to monitoring the temperature and pressure during the reaction. After the reaction is completed, take out the product and cool it to room temperature. Add the product to a 0.5M NaOH solution and etch it at 90℃ for 6 hours. After etching, collect the product by centrifugation and wash it alternately with deionized water and ethanol several times. Place the washed product in an oven and dry it at 80℃ for 12 hours. The dried product is mechanically ground to obtain hollow TiO2 powder. The results are as follows: Due to the reduction in the concentration of the template, the hollow structure formed is less or incomplete, resulting in a decrease in specific surface area and photocatalytic performance.

[0050] Example 2 (Increasing Template Concentration)

[0051] Weigh a certain amount of polyethylene glycol and dissolve it in ethanol to prepare a 0.2M polyethylene glycol solution. Stir it at room temperature for 30 minutes to ensure that the polyethylene glycol is completely dissolved. Slowly add tetrabutyl titanate to the polyethylene glycol solution, keep the stirring speed at 500rpm, and continue stirring for 30 minutes to fully mix the titanium source and the template. Transfer the mixed solution to a hydrothermal reactor, seal it and place it in an oven to react at 150℃ for 6 hours. Pay attention to monitoring the temperature and pressure during the reaction. After the reaction, take out the product and cool it to room temperature. Add the product to a 0.5M NaOH solution and etch it at 90℃ for 6 hours. After etching, collect the product by centrifugation and wash it alternately with deionized water and ethanol several times. Place the washed product in an oven and dry it at 80℃ for 12 hours. The dried product is mechanically ground to obtain hollow TiO2 powder. The results are as follows: Due to the increase in the concentration of the template, more and more complete hollow structures are formed, resulting in an increase in specific surface area and photocatalytic performance.

[0052] Example 3 (lowering the reaction temperature)

[0053] Weigh a certain amount of polyethylene glycol and dissolve it in ethanol to prepare a 0.1M polyethylene glycol solution. Stir it at room temperature for 30 minutes to ensure that the polyethylene glycol is completely dissolved. Slowly add tetrabutyl titanate to the polyethylene glycol solution, keep the stirring speed at 500rpm, and continue stirring for 30 minutes to fully mix the titanium source and the template. Transfer the mixed solution to a hydrothermal reactor, seal it and place it in an oven to react at 130℃ for 6 hours. Pay attention to monitoring the temperature and pressure during the reaction. After the reaction is completed, take out the product and cool it to room temperature. Add the product to a 0.5M NaOH solution and etch it at 90℃ for 6 hours. After etching, collect the product by centrifugation and wash it alternately with deionized water and ethanol several times. Place the washed product in an oven and dry it at 80℃ for 12 hours. The dried product is mechanically ground to obtain hollow TiO2 powder. The results are as follows: lower reaction temperature will lead to incomplete hydrolysis and polycondensation reactions, incomplete hollow structure formation, and affect the specific surface area and photocatalytic performance.

[0054] Example 4 (Increasing the reaction temperature)

[0055] Weigh a certain amount of polyethylene glycol and dissolve it in ethanol to prepare a 0.1M polyethylene glycol solution. Stir it at room temperature for 30 minutes to ensure that the polyethylene glycol is completely dissolved. Slowly add tetrabutyl titanate to the polyethylene glycol solution, keep the stirring speed at 500rpm, and continue stirring for 30 minutes to fully mix the titanium source and the template. Transfer the mixed solution to a hydrothermal reactor, seal it and place it in an oven to react at 170℃ for 6 hours. Pay attention to monitoring the temperature and pressure during the reaction. After the reaction is completed, take out the product and cool it to room temperature. Add the product to a 0.5M NaOH solution and etch it at 90℃ for 6 hours. After etching, collect the product by centrifugation and wash it alternately with deionized water and ethanol several times. Place the washed product in an oven and dry it at 80℃ for 12 hours. The dried product is mechanically ground to obtain hollow TiO2 powder. The results are as follows: Higher reaction temperature promotes hydrolysis and polycondensation reactions, resulting in product agglomeration, which affects the specific surface area and photocatalytic performance.

[0056] Example 5 (Shortening Etching Time)

[0057] Weigh a certain amount of polyethylene glycol and dissolve it in ethanol to prepare a 0.1M polyethylene glycol solution. Stir it at room temperature for 30 minutes to ensure that the polyethylene glycol is completely dissolved. Slowly add tetrabutyl titanate to the polyethylene glycol solution, keep the stirring speed at 500rpm, and continue stirring for 30 minutes to fully mix the titanium source and the template agent. Transfer the mixed solution to a hydrothermal reactor, seal it and place it in an oven to react at 150℃ for 6 hours. Pay attention to monitoring the temperature and pressure during the reaction. After the reaction is completed, take out the product and cool it to room temperature. Add the product to a 0.5M NaOH solution and etch it at 90℃ for 4 hours. After etching, collect the product by centrifugation and wash it alternately with deionized water and ethanol several times. Place the washed product in an oven and dry it at 80℃ for 12 hours. The dried product is mechanically ground to obtain hollow TiO2 powder. The results are as follows: the template is not completely removed due to the short etching time, and the residual template affects the performance of the hollow structure.

[0058] Example 6 (extending etching time)

[0059] Weigh a certain amount of polyethylene glycol and dissolve it in ethanol to prepare a 0.1M polyethylene glycol solution. Stir it at room temperature for 30 minutes to ensure that the polyethylene glycol is completely dissolved. Slowly add tetrabutyl titanate to the polyethylene glycol solution, keep the stirring speed at 500rpm, and continue stirring for 30 minutes to fully mix the titanium source and the template agent. Transfer the mixed solution to a hydrothermal reactor, seal it and place it in an oven to react at 150℃ for 6 hours. Pay attention to monitoring the temperature and pressure during the reaction. After the reaction is completed, take out the product and cool it to room temperature. Add the product to a 0.5M NaOH solution and etch it at 90℃ for 8 hours. After etching, collect the product by centrifugation and wash it alternately with deionized water and ethanol several times. Place the washed product in an oven and dry it at 80℃ for 12 hours. The dried product is mechanically ground to obtain hollow TiO2 powder. The results are: Although a longer etching time can ensure that the template is completely removed, too long etching time destroys the integrity of the hollow structure, resulting in performance degradation.

[0060] The specific surface area and photocatalytic performance are as follows:

[0061]

[0062]

[0063] Table 1

[0064] Based on the data of the experimental group and the control group, we can draw the following conclusions:

[0065] 1. Effect of template concentration:

[0066] When the concentration of the template (PEG) is reduced (as in Example 1), the specific surface area of ​​the hollow TiO2 powder decreases and the photocatalytic performance also decreases slightly. This indicates that the lower template concentration is not enough to form enough hollow structures, or the formed hollow structures are incomplete.

[0067] When the template concentration is increased (such as in Example 2), the specific surface area of ​​the hollow TiO2 powder will increase and the photocatalytic performance will also improve. This is because a higher template concentration is conducive to the formation of more hollow structures, thereby increasing the specific surface area and photocatalytic active sites.

[0068] 2. Effect of hydrothermal reaction temperature:

[0069] Lowering the hydrothermal reaction temperature (such as Example 3) results in incomplete formation of the hollow structure, which in turn reduces the specific surface area and photocatalytic performance. This is because lower temperatures are not conducive to the hydrolysis and polycondensation reactions of the titanium source on the template surface.

[0070] Increasing the hydrothermal reaction temperature (such as Example 4) is helpful for the formation of the hollow structure, but too high a temperature may cause the product to agglomerate, affecting the integrity and performance of the hollow structure. Therefore, it is necessary to find a suitable reaction temperature to obtain the best hollow structure and performance.

[0071] 3. Influence of etching time:

[0072] Shortening the etching time (such as in Example 5) results in the template in the hollow structure not being completely removed, thereby affecting the specific surface area and photocatalytic performance. This is because the etching time is too short to completely remove the template.

[0073] Although extending the etching time (such as in Example 6) can ensure that the template is completely removed, excessive etching may damage the integrity of the hollow structure, resulting in performance degradation. Therefore, it is necessary to optimize the etching time to obtain the best hollow structure and performance.

[0074] In summary, factors such as template concentration, hydrothermal reaction temperature and etching time have an important influence on the performance of hollow TiO2 powders. By adjusting these parameters, the formation and performance of the hollow structure can be optimized.

[0075] When conducting the experiment, the conditions and parameters of each step need to be strictly controlled to ensure the accuracy and reliability of the experimental results. After the experiment, the prepared hollow TiO2 powder can be characterized and analyzed by SEM, TEM, BET, photocatalytic degradation experiments, etc. to verify the correctness of the experimental results.

[0076] This specific embodiment is merely an explanation of the invention and is not a limitation of the invention. After reading this specification, those skilled in the art may make non-creative modifications to this embodiment as needed. However, as long as they are within the scope of protection of the invention, they are protected by patent law.

Claims

1. A process for preparing hollow TiO2 powder, characterized in that: The method comprises a titanium source as a starting material and a surfactant as a template; The preparation process comprises the following steps: Step 1: dissolve the template in a solvent and stir evenly to form a template solution; Step 2: dissolving or dispersing the titanium source in the template solution to form a uniform titanium source-template mixed solution; Step 3: Place the titanium source-template mixed solution into a hydrothermal reactor, seal it, and place it in an oven to react at 150°C for 6 hours to form a TiO2 precursor; Step 4: Place the TiO2 precursor in an extraction solvent to remove the template and obtain hollow TiO2 powder; Step 5: Wash, dry and grind the obtained hollow TiO2 powder.

2. The process for preparing hollow TiO2 powder according to claim 1, characterized in that: The template agent is polyethylene glycol with a concentration of 0.1M.

3. The process for preparing hollow TiO2 powder according to claim 2, characterized in that: The solvent is ethanol and water in a volume ratio of 1:1, and the stirring time in step 1 is 30 minutes and the stirring speed is 500 rpm.

4. The process for preparing hollow TiO2 powder according to claim 3, characterized in that: The titanium source is 0.01-0.05M tetrabutyl titanate, and the volume ratio of the titanium source to the template solution is 1:

10.

5. The process for preparing hollow TiO2 powder according to claim 4, characterized in that: The extraction solvent is acetone. When the TiO2 precursor is placed in acetone to remove the template, the mixed solution of the TiO2 precursor and acetone is stirred for 30 minutes.

6. The process for preparing hollow TiO2 powder according to claim 5, characterized in that: In step 3, when adjusting the pH, ammonia water is used as a regulator to control the pH of the reaction.

7. The process for preparing hollow TiO2 powder according to claim 6, characterized in that: In step 3, the titanium source is stirred during the reaction, and the color gradually changes from transparent to milky white during the stirring process.

8. The process for preparing hollow TiO2 powder according to claim 7, characterized in that: In step 4, the volume ratio of the extraction solvent to the TiO2 precursor is 1:

1.

9. The process for preparing hollow TiO2 powder according to claim 8, characterized in that: In the step 5, the hollow TiO2 powder is ground so that the particle size of the hollow TiO2 powder is 50 nm.

10. The process for preparing hollow TiO2 powder according to claim 9, characterized in that: In step 5, the hollow TiO2 powder is washed and diluted with deionized water.