Preparation method of ferrous sulfate with ultralow magnesium content

By mixing the crude ferrous sulfate with newly prepared ferrous sulfide and ferrous fluoride, condensing and crystallizing after filtration and flocculation, the magnesium content in ferrous sulfate was successfully reduced, and the magnesium content in the prior art was solved. The problem of this has improved the electrical performance of lithium iron phosphate batteries, and the process is simple and cost-effective.

CN118877947APending Publication Date: 2024-11-01SICHUAN JINHENGFENGLING NEW MATERIAL TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410909994.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The prior art is difficult to reduce the magnesium content in ferrous sulfate to a very low level, affecting the electrical performance of lithium iron phosphate batteries.

Method used

The aqueous solution of the crude ferrous sulfate product was mixed with the newly prepared ferrous sulfide and ferrous fluoride, and filtration, flocculation, solid-liquid separation, concentration and crystallization. Through this process, the magnesium content was reduced to below 10 ppm.

Benefits of technology

It achieves extremely low content of magnesium in ferrous sulfate, ensuring the electrical performance of lithium iron phosphate batteries. At the same time, it is simple in process, easy to operate and low cost.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of inorganic chemical industry, in particular to a preparation method of ferrous sulfate with ultralow magnesium content. The invention provides a preparation method of ferrous sulfate with ultralow magnesium content, which comprises the following steps: mixing an aqueous solution of a ferrous sulfate crude product with newly prepared ferrous sulfide, and carrying out first filtration to obtain a first filtrate; mixing the first filtrate with newly prepared ferrous fluoride and a flocculating agent in sequence, and performing flocculation and solid-liquid separation in sequence to obtain a second filtrate; and sequentially concentrating and crystallizing the second filtrate to obtain the ferrous sulfate with ultralow magnesium content. According to the method, the content of the magnesium element in the ferrous sulfate can be removed to an extremely low level below 10ppm; other impurities are not introduced in the technical process; the equipment used in the invention is simple, easy to operate and low in processing cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of inorganic chemical industry, and in particular to a method for preparing ferrous sulfate with ultra-low magnesium content. Background Art

[0002] Ferrous sulfate is the main raw material for introducing iron source in the preparation process of lithium iron phosphate, a new energy material. During the preparation process of lithium iron phosphate, the impurities contained in ferrous sulfate will also be introduced into lithium iron phosphate along with the iron source, thereby affecting the electrical properties of lithium iron phosphate batteries. Therefore, the purification of ferrous sulfate has become a key link in ensuring the quality of lithium iron phosphate. At present, the ferrous sulfate solution is usually impurity-removed by recrystallization, such as the technical solution with patent application number CN202211290879.9, or the ferrous sulfate solution is impurity-removed by sulfide, such as the technical solution with patent application number CN201910256555.5. However, since the water solubility of magnesium compounds and divalent iron compounds is very close, it is difficult for the above-mentioned prior art to reduce the magnesium in ferrous sulfate to a very low level. Summary of the invention

[0003] In order to solve the problems existing in the prior art, the present invention provides a method for preparing ferrous sulfate with ultra-low magnesium content. The ferrous sulfate prepared by the method provided by the present invention can reduce the magnesium content to a very low level.

[0004] In order to achieve the above objectives, the present invention provides the following technical solutions.

[0005] The present invention provides a method for preparing ferrous sulfate with ultra-low magnesium content, comprising the following steps:

[0006] After mixing the aqueous solution of crude ferrous sulfate and freshly prepared ferrous sulfide, a first filtration is performed to obtain a first filtrate;

[0007] The first filtrate is sequentially mixed with freshly prepared ferrous fluoride and a flocculant, and flocculation and solid-liquid separation are sequentially performed to obtain a second filtrate;

[0008] The second filtrate is concentrated and crystallized in sequence to obtain the ferrous sulfate with ultra-low magnesium content.

[0009] Preferably, the method for preparing the newly prepared ferrous sulfide comprises the following steps:

[0010] Sodium sulfide, ferrous sulfate and water are mixed, a first precipitation reaction is carried out, the solid is filtered, and then washed with deionized water to obtain freshly prepared ferrous sulfide.

[0011] Preferably, the method for preparing the newly prepared ferrous fluoride comprises the following steps:

[0012] Dissolving fluoride and ferrous sulfate in water, performing a second precipitation reaction, filtering, and then washing the obtained solid with deionized water to obtain newly prepared ferrous fluoride;

[0013] The fluoride is NaF or ammonium fluoride.

[0014] Preferably, the molar ratio of the fluoride to ferrous sulfate is 1:(1-1.2).

[0015] Preferably, the mass of the newly produced ferrous sulfide is 0.5% to 5% of the mass of the ferrous sulfate in the aqueous solution of the crude ferrous sulfate.

[0016] Preferably, the mass of the newly produced ferrous fluoride is 0.1% to 5% of the mass of the ferrous sulfate in the first filtrate.

[0017] Preferably, the flocculant is polyacrylic acid amide; the mass of the flocculant is 0.1-0.4% of the mass of ferrous sulfate in the first filtrate.

[0018] The present invention provides a method for preparing ferrous sulfate with ultra-low magnesium content, comprising the following steps: after mixing an aqueous solution of crude ferrous sulfate with newly prepared ferrous sulfide, performing a first filtration to obtain a first filtrate; sequentially mixing the first filtrate with newly prepared ferrous fluoride and a flocculant, sequentially performing flocculation and solid-liquid separation to obtain a second filtrate; sequentially concentrating and crystallizing the second filtrate to obtain the ferrous sulfate with ultra-low magnesium content. The present invention can remove the content of magnesium in ferrous sulfate to an extremely low level of less than 10 ppm; other impurities will not be introduced in the process of the present invention; the equipment used in the present invention is simple, easy to operate, and has low processing cost. DETAILED DESCRIPTION

[0019] The present invention provides a method for preparing ferrous sulfate with ultra-low magnesium content, comprising the following steps:

[0020] After mixing the aqueous solution of crude ferrous sulfate and freshly prepared ferrous sulfide, a first filtration is performed to obtain a first filtrate;

[0021] The first filtrate is sequentially mixed with freshly prepared ferrous fluoride and a flocculant, and flocculation and solid-liquid separation are sequentially performed to obtain a second filtrate;

[0022] The second filtrate is concentrated and crystallized in sequence to obtain the ferrous sulfate with ultra-low magnesium content.

[0023] The invention mixes the aqueous solution of crude ferrous sulfate and newly prepared ferrous sulfide, and then performs a first filtration to obtain a first filtrate.

[0024] In the present invention, the mass ratio of the crude ferrous sulfate to water is preferably 1:5-6, more preferably 1:5.5.

[0025] In the present invention, the method for preparing the newly prepared ferrous sulfide preferably comprises the following steps:

[0026] Sodium sulfide, ferrous sulfate and water are mixed, a first precipitation reaction is carried out, the solid is filtered, and then washed with deionized water to obtain freshly prepared ferrous sulfide.

[0027] In the present invention, the sodium sulfide is preferably sodium sulfide nonahydrate; the ferrous sulfate is preferably ferrous sulfate heptahydrate. In the present invention, the molar ratio of the sodium sulfide to the ferrous sulfate is preferably 1:1.

[0028] In the present invention, the mass of the newly produced ferrous sulfide is preferably 0.5% to 5% of the mass of the ferrous sulfate in the aqueous solution of the crude ferrous sulfate, and more preferably 1% to 4%.

[0029] After obtaining the first filtrate, the present invention sequentially mixes the first filtrate with newly prepared ferrous fluoride and a flocculant, and sequentially performs flocculation and solid-liquid separation to obtain a second filtrate.

[0030] In the present invention, the preparation method of the newly prepared ferrous fluoride preferably comprises the following steps:

[0031] Dissolving fluoride and ferrous sulfate in water, performing a second precipitation reaction, filtering, and then washing the obtained solid with deionized water to obtain newly prepared ferrous fluoride;

[0032] The fluoride is NaF or ammonium fluoride.

[0033] In the present invention, the ferrous sulfate is preferably ferrous sulfate heptahydrate. In the present invention, the molar ratio of the fluoride to the ferrous sulfate is preferably 1:1 to 1.2.

[0034] In the present invention, the mass of the newly prepared ferrous fluoride is preferably 0.1% to 5% of the mass of the ferrous sulfate in the first filtrate, and more preferably 2% to 4%. In the present invention, the flocculant is preferably polyacrylic acid amide; the mass of the flocculant is preferably 0.1 to 0.4% of the mass of the ferrous sulfate in the first filtrate.

[0035] In the present invention, the solid-liquid separation method is preferably centrifugation.

[0036] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0037] Example 1

[0038] Take 4.6g (0.019mol) of sodium sulfide nonahydrate crystals and 5.3g (0.019mol) of ferrous sulfate heptahydrate crystals and dissolve them in 100mL of deionized water. After stirring, filter and then wash the obtained solid with deionized water to obtain a newly prepared ferrous sulfide solid.

[0039] 0.22 g (0.005 mol) of NaF and 1.63 g (0.006 mol) of ferrous sulfate heptahydrate crystals were dissolved in 100 mL of deionized water, stirred for 30 min and filtered, and then the obtained solid was washed with deionized water to obtain a freshly prepared ferrous fluoride solid;

[0040] Take 50g of crude ferrous sulfate heptahydrate crystals and dissolve them in 300mL of deionized water, add the aforementioned freshly prepared ferrous sulfide and stir at 300r / min for 30min, add the aforementioned freshly prepared ferrous fluoride solid to the filtrate after filtering, heat to 90°C with stirring and keep for 30min, add 0.1g of polyacrylamide after cooling, flocculate, then centrifuge and filter to obtain a filtrate, and then concentrate and crystallize the filtrate to obtain ferrous sulfate crystals. The magnesium content in the ferrous sulfate crystals is 2ppm as detected by ICP-MS.

[0041] Example 2

[0042] Take 10g (0.04mol) of sodium sulfide nonahydrate crystals and 11.5g (0.04mol) of ferrous sulfate heptahydrate crystals and dissolve them in 150mL of deionized water, stir and filter, then wash the obtained solid with deionized water to obtain a newly prepared ferrous sulfide solid;

[0043] Take 0.5g NaF (0.012mol) and 3.7g ferrous sulfate heptahydrate crystals (0.013mol) and dissolve them in 300mL deionized water, stir for 30min and filter, then wash the obtained solid with deionized water to obtain a freshly prepared ferrous fluoride solid;

[0044] Take 100g of crude ferrous sulfate heptahydrate crystals and dissolve them in 500mL of deionized water, add the aforementioned freshly prepared ferrous sulfide and stir at 300r / min for 30min, add the aforementioned freshly prepared ferrous fluoride solid to the filtrate after filtering, heat to 90°C with stirring and keep for 30min, add 0.15g of polyacrylic acid amide after cooling, flocculate, then centrifuge and filter to obtain a filtrate, and then evaporate the filtrate, concentrate and crystallize to obtain ferrous sulfate crystals. The magnesium content in the ferrous sulfate crystals was detected by ICP-MS to be 3ppm.

[0045] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A method for preparing ferrous sulfate with ultra-low magnesium content, characterized in that: The following steps are involved: After mixing the aqueous solution of crude ferrous sulfate and freshly prepared ferrous sulfide, a first filtration is performed to obtain a first filtrate; The first filtrate is sequentially mixed with freshly prepared ferrous fluoride and a flocculant, and flocculation and solid-liquid separation are sequentially performed to obtain a second filtrate; The second filtrate is concentrated and crystallized in sequence to obtain the ferrous sulfate with ultra-low magnesium content.

2. The method according to claim 1, characterized in that The preparation method of the newly prepared ferrous sulfide comprises the following steps: Sodium sulfide, ferrous sulfate and water are mixed, a first precipitation reaction is carried out, the solid is filtered, and then washed with deionized water to obtain freshly prepared ferrous sulfide.

3. The method according to claim 1, characterized in that The preparation method of the newly prepared ferrous fluoride comprises the following steps: Dissolving fluoride and ferrous sulfate in water, performing a second precipitation reaction, filtering, and then washing the obtained solid with deionized water to obtain newly prepared ferrous fluoride; The fluoride is NaF or ammonium fluoride.

4. The method according to claim 3, characterized in that The molar ratio of the fluoride to ferrous sulfate is 1:(1-1.2).

5. The method according to claim 1, characterized in that The mass of the newly produced ferrous sulfide is 0.5% to 5% of the mass of the ferrous sulfate in the aqueous solution of the crude ferrous sulfate.

6. The method according to claim 1, characterized in that The mass of the newly produced ferrous fluoride is 0.1% to 5% of the mass of the ferrous sulfate in the first filtrate.

7. The method according to claim 1, characterized in that The flocculant is polyacrylic acid amide; the mass of the flocculant is 0.1-0.4% of the mass of ferrous sulfate in the first filtrate.