Nano material based on NiCo-glyceric acid as well as preparation method and application of nano material
Co2NiO4/NiO and CoNi2S4 nanomaterials were prepared by calcining NiCo-glyceric acid as the precursor, and used for the negative electrode of lithium-ion capacitors, which solved the problems of low specific capacity and poor cycle stability of lithium-ion negative electrode materials, and achieved high energy density and high power density Lithium ion capacitor performance.
Patent Information
- Application Number
- CN202410934983.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-01
AI Technical Summary
Existing lithium-ion batteries and supercapacitors cannot meet the needs of high energy density and high power density at the same time, and the specific capacity of lithium-ion negative electrode materials is low and the cycle stability is poor, which affects the performance of energy storage devices.
NiCo-glyceric acid is used as the precursor to prepare Co2NiO4/NiO and CoNi2S4 nanomaterials through calcining process, maintaining the nanospherical structure, and is used for the negative electrode of lithium ion capacitors, and regulating the mass of positive and negative electrode active substances and the voltage window range to optimize performance.
It achieves high specific capacity and good cycle stability, meets the high energy density and high power density requirements of lithium-ion capacitors, and expands the selection range and application fields of negative electrode materials.
Smart Images

Figure CN118877955A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nanomaterials, and in particular to a nanomaterial based on NiCo-glyceric acid and a preparation method and application thereof. Background Art
[0002] The use of new energy storage devices has brought a more convenient way to the conversion and utilization of clean energy, thereby reducing the impact of climate and environmental factors on the use of clean energy. Among the energy storage devices currently used, lithium-ion batteries and supercapacitors have been widely used in small electronic devices, electric vehicles and other fields. However, these two energy storage devices cannot meet the requirements of high energy density and high power density at the same time, so their practical application is limited. Therefore, it is particularly important to develop new energy storage devices that meet the requirements of energy density and power density at the same time. The electrode material used as the negative electrode of lithium-ion capacitors needs to have low lithium insertion potential, high electronic conductivity and fast ion diffusion ability, excellent kinetic process, etc. The negative electrode materials are divided into intercalation type (or embedding type), conversion type and alloy type. Compared with carbides, fluorides and nitrides, transition metal oxides and sulfides have the characteristics of high theoretical specific capacity, abundant reserves and low toxicity, and are new energy storage materials that have received widespread attention. For example, Chinese invention patent CN113745009A discloses a method for preparing a binary nanocomposite material Co3S4 / NiCo2S4 and its application in supercapacitor electrodes, which uses a dual template method combined with a hydrothermal method, specifically including using NiCo-glyceric acid as an initial template, in an aqueous solution, the dissociated cobalt ions are rapidly combined with 2-methylimidazole in the solution, and Co-ZIF is in situ grown on the surface of the NiCo-glyceric acid lipid spheres for modification with 2-methylimidazole, and the obtained Co-ZIF / NiCo-glyceric acid lipid spheres are used as precursors, and then solvent-thermally reacted with thioacetamide. The reaction is carried out, thioacetamide gradually decomposes and generates sulfide ions. Due to the deposition of sulfide ions, the metal ions in the precursor migrate to the surface and generate metal sulfides on the surface of the template, while the template gradually decomposes in the solvent thermal reaction. Finally, it is placed in a tubular furnace for sulfurization reaction to obtain a binary nanocomposite material of Co3S4 / NiCo2S4. The composite material has NiCo2S4 prepared by sulfurizing NiCo-glycerate spheres as the inner core and Co3S4 formed by sulfurizing Co-ZIF as the outer core. It has a complex hollow structure, exhibits good capacitance performance, and can be used as a supercapacitor electrode material.
[0003] Furthermore, the lithium battery negative electrode materials used in the prior art exhibit low specific capacity and poor cycle stability. The electrochemical properties of the negative electrode material are one of the important factors affecting the performance of the energy storage device. Therefore, it is of great significance to develop an electrode material with excellent morphology, high specific capacity and stable cycle.
[0004] In summary, the present invention provides a method of using NiCo-glyceric acid as a precursor, directly treating it by a calcination method, and combining different preparation methods to obtain two nanomaterials, a bimetallic oxide composite and a bimetallic sulfide, which have excellent electrochemical properties and can maintain the spherical morphology of NiCo-glyceric acid. The nanostructures of the bimetallic oxide and the bimetallic sulfide can be designed and applied to the negative electrode of a lithium ion capacitor. By regulating the mass ratio of the positive and negative active substances and the voltage window range, the conditions for regulating the performance of the lithium ion capacitor to reach the optimal state are obtained. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a negative electrode material based on NiCo-glyceric acid and a preparation method and application thereof, which has the advantages of simple process and controllable process, short production time and low cost, and is suitable for large-scale promotion and production.
[0006] In order to achieve the above object, the present invention provides a method for preparing a nanomaterial based on NiCo-glyceric acid, characterized in that the nanomaterial is prepared by using NiCo-glyceric acid as a precursor through a calcination process, and the nanomaterial has the same nano-spherical structure as NiCo-glyceric acid.
[0007] Preferably, the calcination process includes oxidative calcination and sulfidation calcination.
[0008] As a preferred embodiment, the oxidative calcination comprises calcining NiCo-glyceric acid in air, and the NiCo-glyceric acid undergoes an oxidation reaction.
[0009] As a preferred embodiment, the sulfidation calcination comprises calcining NiCo-glyceric acid under the protection of an inert gas, and the NiCo-glyceric acid undergoes a sulfidation reaction.
[0010] In some specific embodiments, the oxidative calcination comprises calcining NiCo-glyceric acid in a muffle furnace at 400-800° C. for 1-5 hours, and the molecular formula of the obtained nanomaterial is Co2NiO4 / NiO.
[0011] Preferably, the nanomaterial obtained after the oxidation and calcination of NiCo-glyceric acid maintains the spherical structure of NiCo-glyceric acid, has a smaller diameter, and has a nano-spherical structure on the surface in which Co2NiO4 and NiO form a heterojunction.
[0012] In some specific embodiments, the sulfidation calcination comprises dissolving NiCo-glyceric acid and thioacetamide in ethanol, and calcining at 200-400° C. for 1-3 hours in a tubular furnace under the protection of an inert gas, and the obtained nanomaterial has a molecular formula of CoNi2S4.
[0013] Preferably, the mass ratio of glyceric acid to thioacetamide is 1:1 to 1:3;
[0014] Preferably, the nanomaterial obtained after the sulfurization and calcination of NiCo-glyceric acid has a nano-spherical structure with a constant diameter and a rough surface and a hollow structure.
[0015] Preferably, the inert gas is selected from nitrogen or argon.
[0016] Preferably, the precursor is prepared by a solvothermal method, wherein the nickel source and the cobalt source are respectively dissolved in a mixed solution of isopropanol and glycerol, stirred evenly, and then heated at 180° C. for 6 h to obtain NiCo-glyceric acid.
[0017] As another object, the present invention also provides nanomaterials obtained by the above-mentioned preparation method, including Co2NiO4 / NiO composite nanomaterials and CoNi2S4 nanomaterials.
[0018] As one of the purposes of the invention, the nanomaterial provided by the above technical solution is used as a negative electrode material in a lithium ion capacitor.
[0019] Compared with the prior art, the beneficial technical effects obtained by the present invention are:
[0020] (1) The technical solution of the present invention is used to oxidize and sulfurize the NiCo-G precursor based on its nano-spherical morphology. On the one hand, the obtained nanomaterial maintains the morphology of the precursor, wherein Co2NiO4 and NiO in the Co2NiO4 / NiO solid nanosphere material form a heterojunction structure, which can effectively improve the conductivity of the negative electrode material; on the other hand, the CoNi2S4 hollow structure obtained after sulfurization calcination has a larger specific surface area, thereby increasing the contact area between the negative electrode material and the electrolyte and shortening the ion transmission distance; therefore, the nanomaterial provided by the technical solution of the present invention can be applied to lithium ion capacitors and has good specific capacity and cycle stability.
[0021] (2) When the nanomaterial provided by the technical solution of the present invention is used as the negative electrode material of the lithium ion capacitor, it can meet the requirements of the lithium ion capacitor to have high specific capacity, low discharge platform and excellent long cycle stability. In addition, based on the fact that the high-performance lithium ion capacitors in the prior art are faced with the problem of poor performance caused by the mismatch between the positive and negative electrodes, the present invention solves this problem by adjusting the voltage window and the amount of active substances. The present invention also explores the effects of different positive and negative electrode active material loadings and voltage window ranges on the performance of lithium ion capacitors, and obtains the optimal positive and negative electrode active material loadings and voltage window ranges. The present invention not only expands the selection range of lithium storage negative electrode materials, but also expands the application fields of the above two materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is a flow chart for preparing Co2NiO4 / NiO and CoNi2S4 nanomaterials of Examples 1 and 2 of the present invention.
[0023] Figure 2a-2b This is the XRD spectrum and EDS spectrum of the Co2NiO4 / NiO nanomaterial provided in Example 1 of the present invention.
[0024] Figure 2c-2d This is the XRD spectrum and EDS spectrum of the CoNi2S4 nanomaterial provided in Example 2 of the present invention.
[0025] Figure 3a It is a comparison chart of N2 adsorption and desorption curves of Example 1 and Example 2 of the present invention and NiCo-G precursor.
[0026] Figure 3b It is a comparison chart of the specific surface areas of Example 1 and Example 2 of the present invention and the NiCo-G precursor.
[0027] Figure 4a-4c These are SEM and TEM images of the NiCo-G precursor prepared in Example 1 of the present invention at different magnifications.
[0028] Figure 4d-4f These are SEM and TEM images of Co2NiO4 / NiO prepared in Example 1 of the present invention at different magnifications.
[0029] Figure 4g-Figure 4i These are SEM and TEM images of CoNi2S4 prepared in Example 2 of the present invention at different magnifications.
[0030] Figure 4j This is a particle size distribution diagram of the NiCo-G precursor prepared in Example 1 of the present invention.
[0031] Figure 4k This is the particle size distribution diagram of Co2NiO4 / NiO prepared in Example 1 of the present invention.
[0032] Figure 4l CoNi2S prepared in Example 2 of the present invention 4的 Particle size distribution diagram.
[0033] Figure 5a The Co2NiO4 / NiO provided in Example 1 of the present invention is 0.1Ag -1 Lower cycle performance test diagram.
[0034] Figure 5b This is a rate performance test diagram of Co2NiO4 / NiO at different circuit densities provided in Example 1 of the present invention.
[0035] Figure 5c The CoNi2S4 provided in Example 2 of the present invention is in 0.1Ag -1 Lower cycle performance test diagram.
[0036] Figure 5d This is a long cycle performance test chart of CoNi2S4 provided in Example 2 of the present invention at 2A / g.
[0037] Figure 6a CV cyclic voltammetry curves of the positive electrode material activated carbon AC (YP-80) at different scan rates in Example 3 of the present invention;
[0038] Figure 6b This is a rate performance diagram of the positive electrode material activated carbon AC (YP-80) AC in Example 3 of the present invention.
[0039] Figure 6c-6d The positive electrode material AC (YP-80) in Example 3 of the present invention is respectively 1Ag -1 and 2Ag -1 The long cycle performance test diagram below.
[0040] Figure 7a Schematic diagram of the simulated structure of Co2NiO4 / NiO / / AC and CoNi2S4 / / AC lithium ion capacitors assembled using the nanomaterials of Example 1 and Example 2 as negative electrode materials and graphite as positive electrode materials in Example 3 and Example 4 of the present invention respectively.
[0041] Figure 7b CV curves of the Co2NiO4 / NiO / / AC lithium ion capacitor assembled in Example 3 of the present invention at different voltage windows.
[0042] Figure 7c This is a comparison chart of the specific capacitance of the Co2NiO4 / NiO / / AC lithium ion capacitor assembled in Example 3 of the present invention at different current densities with different positive and negative electrode active material loadings.
[0043] Figure 7d The Co2NiO4 / NiO / / AC lithium ion capacitor assembled in Example 3 of the present invention is 1Ag -1 The long cycle performance test diagram below.
[0044] Figure 7e CV curves of the CoNi2S4 / / AC lithium ion capacitor assembled in Example 4 of the present invention under different voltage windows.
[0045] Figure 7fThis is a comparison chart of the specific capacitance of the CoNi2S4 / / AC lithium ion capacitor assembled in Example 4 of the present invention at different current densities with different positive and negative electrode active material loadings.
[0046] Figure 7g The CoNi2S4 / / AC lithium ion capacitor assembled in Example 4 of the present invention is 1Ag -1 The long cycle performance test diagram below.
[0047] Figure 8 Ragon diagrams of Co2NiO4 / NiO / / AC and CoNi2S4 / / AC lithium ion capacitors at different loading ratios of positive and negative active materials in Examples 3 and 4 of the present invention. DETAILED DESCRIPTION
[0048] In order to make the purpose, technical solutions and advantages of the embodiments of the present application clearer, the technical solutions in the embodiments of the present application will be clearly and completely described below in combination with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments.
[0049] In the present invention, firstly, a solid spherical material with a nanostructure is selected from the precursor of the material, and two electrode materials, Co2NiO4 / NiO and CoNi2S4, are prepared by high-temperature oxidation and sulfurization, respectively, which inherit the morphology and structure of the precursor. Due to different processing techniques, Co2NiO4 / NiO exhibits smaller solid nanospheres, while CoNi2S4 is a hollow spherical structure with a similar size to NiCo-G. Co2NiO4 / NiO and CoNi2S4 exhibit high specific capacity when used as negative electrode materials, at 0.1Ag -1 The maximum current density can reach 1362.5 mAh g -1 . Lithium-ion capacitors were assembled with Co2NiO4 / NiO and CoNi2S4 as negative electrodes and AC as positive electrodes. By adjusting the voltage window and changing the ratio of the loading amount of positive and negative active substances, lithium-ion capacitors with high power density and high energy density were assembled. The successful synthesis of these two materials and their excellent electrochemical properties have laid the foundation for their application in energy storage. At the same time, in order to solve the problem of mismatch between the positive and negative electrodes of lithium-ion capacitors, the present invention uses a method that combines voltage window matching and positive and negative active substance mass matching, which provides new ideas and methods for the problem of matching the positive and negative electrodes of lithium-ion capacitors.
[0050] See also Figure 1, which is a preparation flow chart of the present invention for preparing Co2NiO4 / NiO and CoNi2S4 nanomaterials, first, NiCo-glyceric acid (NiCo-G) was prepared by a solvothermal method, and then Co2NiO4 / NiO and CoNi2S4 were prepared respectively using NiCo-G as a precursor. The preparation process of NiCo-glyceric acid is as follows: 0.1mmol Ni(NO3)2·6H2O and 1.43gCo(NO3)2·6H2O were dissolved in a mixed solution of 8mL glycerol and 40mL isopropanol, stirred for 30min under magnetic stirring at 600r / min, and then transferred into a 100mL reactor and heated at 180℃ for 6h to obtain NiCo-G.
[0051] NiCo-G was placed in a muffle furnace and calcined at 500°C for 2 h to obtain Co2NiO4 / NiO composite nanomaterials with a heterogeneous structure.
[0052] 30 mg of NiCo-G and 50 mg of thioacetamide were dissolved in 30 ml of ethanol and transferred to a 50 ml reactor to react at 160 °C for 1 h. The obtained product was calcined in a tubular furnace at 300 °C for 2 h to obtain CoNi2S4.
[0053] It should be noted that, unless otherwise specified, the raw materials and chemical reagents used in the present invention are all commercially available.
[0054] The technical solutions in the embodiments of the present invention are clearly and completely described below through specific embodiments and drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0055] Example 1
[0056] This embodiment provides a method for preparing a Co2NiO4 / NiO composite nanomaterial, and the specific steps include:
[0057] 1. Provide NiCo-G precursor solution;
[0058] 0.02910g Co(NO3)·6H2O and 0.05816g Ni(NO3)·6H2O were dissolved in a mixed solution of 8mL glycerol and 40mL isopropanol, stirred at a magnetic stirring speed of 500r / min for 40 minutes, and then the mixed solution was poured into a 100mL polytetrafluoroethylene reactor and heated at 120, 150, 180℃ and 200℃ for 4, 6, 8, and 10 hours respectively. After cooling to room temperature, it was washed with anhydrous ethanol 6 times and finally placed in a vacuum drying oven at 60℃ overnight to obtain NiCo-G. It was finally determined that the optimal solvent thermal reaction temperature for the preparation of NiCo-G was 180℃ and the optimal reaction time was 6h.
[0059] 2. Provide Co2NiO4 / NiO composite nanomaterials
[0060] Place 100 mg CoNi-G (180°C, 6h) provided in step 1 into a porcelain boat, then transfer it to a muffle furnace and calcine in air at 300, 400, 500 and 600°C for 1, 2, 3 and 4h (both the heating rate and the cooling rate are 3°C / min), respectively, to obtain Co2NiO4 / NiO material; determine the optimal calcination temperature to be 500°C; and the optimal calcination time to be 3h.
[0061] Example 2
[0062] This embodiment provides a method for preparing CoNi2S4 nanomaterials, and the specific steps include:
[0063] In 30mL ethanol solution, 30mg CoNi-G (180℃, 6h) was mixed with 50mg thioacetamide (TAA). The mixture was magnetically stirred at 500r / min for 30min to ensure thorough dispersion. Subsequently, the homogenized mixture was transferred to a 50ml reactor. In the reactor, the mixture was heated at 120, 140, 160, 180, and 200℃, respectively, with heating times of 0.5, 1, and 2h, respectively. After cooling to room temperature, it was centrifugally washed 6 times with anhydrous ethanol, and then dried overnight at 60℃ in a vacuum drying oven to obtain CoNi2S4 material; it was finally determined that the optimal heating temperature for preparing CoNi2S4 was 160℃, and the optimal heating time was 1h.
[0064] Example 3
[0065] Co2NiO4 / NiO / / AC lithium ion capacitor was assembled with Co2NiO4 / NiO as negative electrode material and activated carbon AC as positive electrode material. The electrolyte was 1M LiPF6 (dissolved in a mixture of ethylene carbonate, diethyl carbonate and dimethyl carbonate in a volume ratio of 1:1:1), and the separator was Celgard 2500. Figure 7a, which is a schematic diagram of the assembly process of Co2NiO4 / NiO / / AC lithium-ion capacitor.
[0066] The Co2NiO4 / NiO / / AC lithium-ion capacitor was assembled in a glove box (O2 content <0.01ppm). Before assembly, the Co2NiO4 electrodes needed to be assembled into half-cells and cycled for 5 to 10 cycles at a current density of 0.1A / g for pre-lithiation.
[0067] The specific assembly process of lithium-ion capacitors is as follows: first, the CoF2 electrode sheet with pre-lithium embedded active material thickness of 50 to 250 μm is taken out from the half-cell, and then it is placed in the negative electrode shell as the negative electrode, and the electrolyte (1M LiPF6) is dripped into it. Then, the diaphragm (Celgard 2400) is placed, the electrolyte is dripped into it, and the positive electrode sheet with active material thickness of 50 to 250 μm is placed in it. Finally, the gasket, shrapnel, and positive electrode shell are placed in turn, and they are packed in a sealed bag and taken out of the glove box. Finally, they are packaged with a packaging machine and left to stand for 12 hours.
[0068] After assembly, the electrochemical performance of the Co2NiO4 / NiO / / AC lithium-ion capacitor was tested. The instruments needed for the test were the electrochemical workstation CHI660e (Shanghai Chenhua) and the Blue Electric tester (Wuhan Blue Electric Electronics Co., Ltd.). The electrochemical workstation CHI660e is used to test the voltage window range, specific capacitance and constant current charge and discharge curve of the lithium-ion capacitor, and the Blue Electric tester is used to test the long cycle performance of the lithium-ion capacitor at a high current density.
[0069] Parameter selection: Set the voltage windows to 0.2-3.2V, 0.2-3.4V, 0.2-3.6V, 0.2-3.8V, 0.2-4.0V, 0.2-4.2V, 0.2-4.3V and 0.2-4.5V respectively; at the same time, control the mass ratio of the active substances of the positive and negative electrodes to 1:1.0, 1:1.5 and 1:2.0 respectively for electrochemical performance testing.
[0070] Finally, considering the electrode polarization, electrolyte decomposition voltage and electrochemical performance, the optimal voltage window of Co2NiO4 / NiO / / AC was determined to be 0.2-4.3V. Based on the comparison of the electrochemical performance of the assembled lithium ion capacitor, the optimal ratio of the positive and negative active materials of Co2NiO4 / NiO / / AC was determined to be 1:1 (see Figure 7c ).
[0071] Example 4
[0072] The difference between this embodiment and embodiment 3 is that this embodiment uses CoNi2S4 as the negative electrode material, activated carbon AC as the positive electrode material to assemble a lithium ion capacitor, the electrolyte is 1M LiPF6 (dissolved in a mixture of ethylene carbonate, diethyl carbonate and dimethyl carbonate in a volume ratio of 1:1:1), and the diaphragm is Celgard 2500. Figure 7a , which is a schematic diagram of the assembly process of CoNi2S4 / / AC lithium-ion capacitor.
[0073] The CoNi2S4 / / AC lithium-ion capacitor is assembled in a glove box (O2 content <0.01ppm). Before assembly, the Co2NiO4 electrodes need to be assembled into half-cells and cycled for 5 to 10 cycles at a current density of 0.1A / g for pre-lithiation.
[0074] The specific assembly process of lithium-ion capacitors is as follows: first, the CoF2 electrode sheet with pre-lithium embedded active material thickness of 50 to 250 μm is taken out from the half-cell, and then it is placed in the negative electrode shell as the negative electrode, and the electrolyte (1M LiPF6) is dripped into it. Then, the diaphragm (Celgard 2400) is placed, the electrolyte is dripped into it, and the positive electrode sheet with active material thickness of 50 to 250 μm is placed in it. Finally, the gasket, shrapnel, and positive electrode shell are placed in turn, and they are packed in a sealed bag and taken out of the glove box. Finally, they are packaged with a packaging machine and left to stand for 12 hours.
[0075] The electrochemical performance of the CoNi2S4 / / AC lithium-ion capacitor was tested after assembly.
[0076] Parameter selection: Set the voltage windows to 0.2-3.2V, 0.2-3.4V, 0.2-3.6V, 0.2-3.8V, 0.2-4.0V, 0.2-4.2V, 0.2-4.3V and 0.2-4.5V respectively, and control the mass ratio of active substances of positive and negative electrodes to 1:1.0, 1:1.5 and 1:2.0.
[0077] Finally, considering the electrode polarization, electrolyte decomposition voltage and electrochemical performance, the optimal voltage window of CoNi2S4 / / AC was determined to be 0.2-4.0 V. Based on the comparison of the performance of the assembled lithium-ion capacitors, the optimal ratio of the positive and negative active materials of CoNi2S4 / / AC was determined to be 1:2.
[0078] Morphology and performance characterization:
[0079] See also Figure 2a-2d The XRD patterns and EDS patterns of Co2NiO4 / NiO and CoNi2S4 prepared in Example 1 and Example 2 of the present invention are shown in the figure. Figure 2aThe XRD pattern of the synthesized Co2NiO4 / NiO is basically corresponding to the standard cards of Co2NiO4 and NiO, proving the successful synthesis of Co2NiO4 / NiO; Figure 2b The EDS results in show that the atomic ratio is about 1:2:4; Figure 2c The XRD pattern of CoNi2S4 is completely consistent with the standard card, proving the successful synthesis of CoNi2S4; Figure 2d This is the EDS spectrum of CoNi2S4, whose atomic ratio is approximately 1:2:4.
[0080] Specific surface area (SSA) is one of the factors that affect the electrochemical properties of materials. Therefore, the present invention also conducts comparative analysis on the changes in specific surface areas of NiCo-G, Co2NiO4 / NiO and CoNi2S4 after conversion, and uses BET to test the specific surface areas of the materials respectively; Figure 3a It can be seen that the specific surface areas of CoNi-G, Co2NiO4 / NiO and CoNi2S4 are 360.97, 8.97 and 38.16 m 2 g -1 ;like Figure 3b As shown in the figure, due to the disappearance of most of the micropores in NiCo-G after oxidation and sulfidation, the specific surface areas of Co2NiO4 / NiO and CoNi2S4 are significantly reduced, and the pore size distribution of Co2NiO4 / NiO and CoNi2S4 is mainly dominated by mesopores.
[0081] Furthermore, the present invention also uses scanning electron microscopy (SEM) and transmission electron microscopy (TEM) to observe the morphology and structure of the precursors NiCo-G, Co2NiO4 / NiO and CoNi2S4. Figure 4a-Figure 4i , respectively, SEM and TEM images of NiCo-G, Co2NiO4 / NiO and CoNi2S4 at different magnifications; specifically, Figure 4a-4c The results of scanning electron microscopy and transmission electron microscopy at different magnifications showed that the prepared precursor NiCo-G was a solid sphere with uniform morphology and smooth surface, and its diameter was about 471.5±70.5nm.
[0082] Figure 4d-4f Shown is the Co2NiO4 / NiO composite obtained after oxidation of NiCo-G, which has the same shape as a solid sphere.
[0083] like Figure 4g-Figure 4i As shown, CoNi-G transforms into CoNi2S4 nanomaterials after sulfurization, and its morphology changes into nanospheres with a rough surface and a hollow structure.
[0084] Further, see Figure 4j-Figure 4lThe particle size distribution diagrams of the NiCo-G precursor, Co2NiO4 / NiO composite material and CoNi2S4 nanomaterial prepared in Example 1 and Example 2 respectively; Figure 4j It can be seen that the particle size of NiCo-G precursor is mainly distributed in 471.5±70.5nm; Figure 4k It can be seen that the particle size distribution of Co2NiO4 / NiO composite material is mainly 253.6±51.0nm; Figure 4l It can be seen that the particle sizes of CoNi2S4 nanomaterials are 490±90nm.
[0085] In summary, it can be seen that the diameter of CoNi2S4 nanomaterial (471.5±70.5nm) is almost unchanged compared with the diameter of NiCo-G (about 490±90nm), while the diameter of Co2NiO4 / NiO composite material is significantly smaller.
[0086] Figure 3a-Figure 3b BET results and Figure 4a-Figure 4i The results of SEM and TEM images of Co2NiO4 / NiO and CoNi2S4 nanomaterials shown are consistent.
[0087] Furthermore, the present invention tested the electrochemical properties of the capacitors assembled in Example 3 and Example 4, and the specific results are shown in Figure 5a-5d .
[0088] like Figure 5a As shown, Co2NiO4 / NiO electrode at 0.1Ag -1 The maximum specific capacity can reach 1260.9 mAh g at a current density of 165 cycles. -1 In the figure, Charge means charging, Discharge means discharging, and Coulombic Efficiency means Coulombic efficiency.
[0089] like Figure 5b As shown, at current densities of 0.1, 0.2, 0.5, 1.0, 2.0 and 4.0Ag -1 When the specific capacities of Co2NiO4 / NiO are maintained at 832.9, 531.7, 262.7, 193.8, 121.9 and 63.2 mAh g -1 When the current density returns to 0.1Ag -1 Its maximum specific capacity can reach 1362.5 mAh g -1 .
[0090] like Figure 5c As shown, CoNi2S4 at 0.1A g -1The long cycle under the condition is similar to that of Co2NiO4 / NiO, and the specific capacity can reach 495.0mAh g after 570 cycles. -1 .
[0091] Figure 5d As shown, the specific capacity of CoNi2S4 is 2Ag -1 After 3000 cycles, it can reach 211.1mAh g -1 .
[0092] Depend on Figure 5a-Figure 5b Comparison of the electrochemical properties of CoNi2S4 and Co2NiO4 / NiO revealed that both samples derived from NiCo-G spheres have high specific capacity and excellent long-cycle performance, showing great potential as high-performance lithium-ion capacitor anodes. However, the initial structure of CoNi2S4 with a hollow structure collapses severely, resulting in a large irreversible capacity. Although these irreversible chemical reactions will gradually be activated to release capacity with cycling, this large capacity decay is not conducive to electrode applications. In contrast, Co2NiO4 / NiO solid spheres with smaller sizes and heterojunctions can better resist the effects of volume changes on electrochemical performance, and the enhanced heterojunction interface formed by Co2NiO4 and NiO can improve electronic conductivity and accelerate electron transport.
[0093] See also Figure 6a and Figure 6b The electrochemical performance of AC (YP80) was tested for the activated carbon used as the positive electrode material in Examples 3 and 4. Figure 6a As shown in the CV (Current-Voltage Potential) curve, activated carbon has excellent cycle stability and capacitance performance for AC (YP80), such as Figure 6b As shown, at 1Ag -1 and 2A g -1 The specific capacity at the current density can reach 60mAh g -1 and 40mAh g -1 .
[0094] See also Figure 7b-7g , are the electrochemical test results of Co2NiO4 / NiO / / AC and CoNi2S4 / / AC lithium ion capacitors of Example 3 and Example 4, respectively.
[0095] See also Figure 7b and Figure 7eBy measuring the CV curves of lithium ion capacitors at different voltage windows at the same scan rate, it was determined that the optimal voltage windows of Co2NiO4 / NiO / / AC and CoNi2S4 / / AC were 0.2-4.3V and 0.2-4.0V, respectively.
[0096] Furthermore, the present invention also investigates the effect of active material loading on the performance of lithium ion capacitors, and the electrochemical characteristics of Co2NiO4 / NiO / / AC and CoNi2S4 / / AC lithium ion capacitors when the mass ratio of the active material loading of the anode material and the cathode material are 1:1.0, 1:1.5 and 1:2.0, respectively.
[0097] like Figure 7c As shown, the specific capacitance of Co2NiO4 / NiO / / AC lithium ion capacitor is the largest when the active material loading is 1:1.0, and ... -1 The specific capacitances are 49.1, 47.5, 45.6, 42.7, 38.9, 36.7, 27.8, 21.5, 16.2, 11.2 and 6.7 F g -1 Unlike Co2NiO4 / NiO / / AC, CoNi2S4 / / AC showed a significant decrease in the active material loading at 0.05, 0.1, 0.2, 0.5, 1, 2, 4, 6, 8, 10, and 12 Ag when the active material loading was 1:2.0. -1 The specific capacitances are 36.7, 32.1, 30.1, 27.9, 26.1, 23.3, 19.0, 15.6, 12.2, 9.7 and 6.9 F g, respectively. -1 ,like Figure 7f shown.
[0098] Furthermore, participation Figure 7d and Figure 7g , in order to test the cycling stability of Co2NiO4 / NiO / / AC and CoNi2S4 / / AC lithium ion capacitors by electrochemical methods, the capacity retention rates after 5000 cycles reached 82.2% and 73.3%, respectively.
[0099] Based on the above comparison results of the positive and negative electrode active material loading, the maximum energy density test was also carried out, see Figure 8 , which is the Ragon diagram of Co2NiO4 / NiO / / AC and CoNi2S4 / / AC when the mass ratios of the positive and negative electrode active materials in the Co2NiO4 / NiO / / AC and CoNi2S4 / / AC lithium ion capacitors in Example 3 and Example 4 are 1:1.0, 1:1.5 and 1:2.0 respectively.
[0100] Figure 8 It shows that the maximum energy density of Co2NiO4 / NiO / / AC and CoNi2S4 / AC reaches 114.6Wh kg -1 (102.5W kg -1 Hours) and 73.6Wh kg -1 (95W kg- 1 When the power density is 20.5kW kg -1 and 19.0kW kg -1 When the energy density is maintained at 26.1Wh kg -1 and 19.5Wh kg -1 .
[0101] Based on the above analysis, the present invention uses NiCo-G with a nano-spherical structure as a precursor, and prepares nanomaterials with different structures of Co2NiO4 / NiO nano-solid spheres and CoNi2S4 nano-hollow spheres through two different calcination processes of high-temperature oxidation and sulfurization, and uses them as negative electrodes of lithium-ion capacitors. In addition, the matching problem of lithium-ion capacitors is explored by adjusting the voltage window and the ratio of the amount of active substances of the positive and negative electrodes.
[0102] The various aspects, embodiments, features and examples of the present invention should be considered as illustrative in all aspects and are not intended to limit the present invention, the scope of the present invention is defined only by the claims. Other embodiments, modifications and uses will be apparent to those skilled in the art without departing from the spirit and scope of the claimed invention.
[0103] Use of title and description in this invention
[0104] It is not meant to limit the invention; each section may apply to any aspect, embodiment or feature of the invention.
[0105] Throughout the present disclosure, where a composition is described as having, comprising, or including particular components, or where a process is described as having, comprising, or including particular process steps, it is contemplated that the compositions taught by the present invention also consist essentially of, or consist of, the recited components, and that the processes taught by the present invention also consist essentially of, or consist of, the recited process steps.
[0106] Unless specifically stated otherwise, use of the terms "include," "includes," "including," "have," "has," or "having" should generally be construed as open ended and non-limiting.
[0107] It should be understood that the order of the various steps or the order in which a particular action is performed is not very important, as long as the teachings of the present invention remain operable. In addition, two or more steps or actions may be performed simultaneously.
[0108] In addition, the inventors of this case also referred to the aforementioned embodiments and conducted experiments with other raw materials, process operations, and process conditions described in this specification, and obtained relatively ideal results.
[0109] Although the present invention has been described with reference to illustrative embodiments, it will be appreciated by those skilled in the art that various other changes, omissions and / or additions may be made without departing from the spirit and scope of the present invention and that the elements of the embodiments may be replaced by substantial equivalents. In addition, many modifications may be made without departing from the scope of the present invention to adapt specific circumstances or materials to the teachings of the present invention. Therefore, it is not intended herein to limit the present invention to the disclosed specific embodiments for performing the present invention, but it is intended that the present invention will include all embodiments within the scope of the appended claims. In addition, unless specifically stated, any use of the terms first, second, etc. does not indicate any order or importance, but rather uses the terms first, second, etc. to distinguish one element from another.
Claims
1. A method for preparing a nanomaterial based on NiCo-glyceric acid, characterized in that: The nano material is prepared by using NiCo-glyceric acid as a precursor through a calcination process, and the nano material has the same nano spherical structure as that of NiCo-glyceric acid.
2. The preparation method according to claim 1, characterized in that: The calcination process includes oxidation calcination and sulfidation calcination; The oxidation calcination comprises calcining NiCo-glyceric acid in air, and the NiCo-glyceric acid undergoes an oxidation reaction; The sulfidation calcination comprises calcining NiCo-glyceric acid under the protection of an inert gas, and the NiCo-glyceric acid undergoes a sulfidation reaction.
3. The preparation method according to claim 1, characterized in that: The oxidation calcination comprises calcining NiCo-glyceric acid in a muffle furnace at 400-800°C for 1-5h, and the molecular formula of the obtained nano material is Co2NiO4 / NiO; And / or, the sulfidation calcination comprises dissolving NiCo-glyceric acid and thioacetamide in ethanol, and calcining at 200-400° C. for 1-3 hours in a tubular furnace under the protection of an inert gas, and the obtained nanomaterial has a molecular formula of CoNi2S4.
4. The preparation method according to claim 3, characterized in that: The nano material obtained after the oxidation and calcination of NiCo-glyceric acid maintains the spherical structure of NiCo-glyceric acid, has a smaller diameter, and has a nano spherical structure on the surface where Co2NiO4 and NiO form a heterojunction; The nano material obtained after the NiCo-glyceric acid is subjected to the sulfurization and calcination has a nano spherical structure with a constant diameter and a rough surface and a hollow structure.
5. The preparation method according to claim 3, characterized in that: The mass ratio of glyceric acid to thioacetamide is (1:1) to (1:3); The inert gas is selected from nitrogen or argon.
6. The preparation method according to any one of claims 1 to 5, characterized in that: The precursor adopts a solvothermal method, wherein a nickel source and a cobalt source are respectively dissolved in a mixed solution of isopropanol and glycerol, stirred evenly, and then heated at 180° C. for 6 hours to obtain NiCo-glyceric acid.
7. The nanomaterial obtained by the preparation method according to any one of claims 1 to 6, comprising Co2NiO4 / NiO composite nanomaterial and CoNi2S4 nanomaterial.
8. A negative electrode material for a lithium ion capacitor, comprising the nanomaterial according to claim 7; When the current density is 0.1A g -1 When the negative electrode material has a maximum specific capacity of 1362.5 mAh g -1 .
9. A lithium ion capacitor, comprising at least the nanomaterial as claimed in claim 7 as a negative electrode material and activated carbon AC as a positive electrode material.
10. The lithium ion capacitor according to claim 9, characterized in that: When the negative electrode material is a Co2NiO4 / NiO composite nanomaterial, the mass ratio of the active material loading amount of the negative electrode material to the positive electrode material is 1:1 to 1:2; When the negative electrode material is CoNi2S4 nanomaterial, the mass ratio of the active material loading amount of the negative electrode material to that of the positive electrode material is 1:1N1:2; The capacity retention rates of Co2NiO4 / NiO / / AC lithium ion capacitors and CoNi2S4 / / AC lithium ion capacitors after 5000 cycles are 82.2% and 73.3%, respectively.