Capacitive deionization positive electrode, capacitive deionization negative electrode and capacitive deionization device

By using amino-modified activated carbon and sulfonic acid-modified activated carbon in capacitor deionized electrodes, the grafting rate is controlled to improve the ion removal rate and cyclic performance of the electrodes, the problem of short life of the capacitor deionization technology is solved and more efficient ion removal and longer service life.

CN118878019APending Publication Date: 2024-11-01FOSHAN SHUNDE MIDEA WATER DISPENSER MFG +1

Patent Information

Application Number
CN202411274366.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing capacitive deionization technology has a short lifespan in water purification, and cannot effectively retain mineral ions that are beneficial to the human body, and it is difficult to effectively remove heavy metal ions.

Method used

The amino-modified activated carbon is used as the positive electrode active material and the sulfonic acid-modified activated carbon is used as the negative electrode active material. By controlling the grafting rate of amino and sulfonic acid groups between 20%~75% and 10%~60%, respectively. Improve the ion removal rate and cycling performance of the positive and negative electrodes, and extend the electrode life.

Benefits of technology

It significantly improves the ion removal rate and cycling performance of the electrode, extends the service life of the electrode, and effectively adsorbs negative and positive ions, enhancing the capture ability of the electrode and shielding the same-ion effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118878019A_ABST
    Figure CN118878019A_ABST
Patent Text Reader

Abstract

The invention provides a capacitive deionization positive electrode, a capacitive deionization negative electrode and a capacitive deionization device. The capacitive deionization positive electrode comprises a first current collector and a positive active material layer, the positive active material layer is adjacent to at least one side of the first current collector, the positive active material layer comprises amino-modified activated carbon, and the grafting rate of amino of the amino-modified activated carbon is 20%-75%. By adopting the positive electrode provided by the invention, the ion removal rate can be improved, and the positive electrode has a relatively long service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of water treatment, and in particular to a capacitor deionization positive electrode, a capacitor deionization negative electrode and a capacitor deionization device. Background Art

[0002] In household water use, the current mainstream solutions for filtering out charged ions in water include ultrafiltration, nanofiltration, and reverse osmosis. Among them, reverse osmosis technology has become the market's first choice for its excellent filtration effect (99%), but the same problem is that with the improvement of people's awareness of drinking water and their concern for health, the water effluent from reverse osmosis is too pure and does not retain mineral ions that are beneficial to the human body. Therefore, the application of capacitive deionization technology that retains ions in water purification scenarios has received more and more research. Capacitive deionization technology can achieve different effluent water qualities at different voltages, while retaining ions that are beneficial to the human body and removing heavy metal ions. However, the current problem of short lifespan limits its further application in water purification. Summary of the invention

[0003] The present invention aims to solve one of the technical problems in the prior art at least to a certain extent. To this end, one object of the present invention is to provide a capacitor deionization positive electrode, a capacitor deionization negative electrode and a capacitor deionization device.

[0004] In a first aspect of the present invention, the present invention provides a capacitor deionization positive electrode. According to an embodiment of the present invention, the capacitor deionization positive electrode comprises a first current collector and a positive electrode active material layer, the positive electrode active material layer is adjacent to at least one side of the first current collector, the positive electrode active material layer comprises amino-modified activated carbon, and the grafting rate of amino groups of the amino-modified activated carbon is 20% to 75%.

[0005] According to the above embodiment of the present invention, the capacitor deionization positive electrode comprises a first current collector and a positive electrode active material layer, the positive electrode active material layer is adjacent to at least one side of the current collector, and the positive electrode active material layer comprises amino-modified activated carbon, the amino modification enriches the surface groups of the activated carbon, can make full use of the specific surface area of ​​the activated carbon, improve the utilization rate of the activated carbon, and at the same time, the amino modification improves the wettability of the activated carbon surface with electrolytic water, reduces the diffusion resistance of ions in the activated carbon electrode, and improves the conductivity of the activated carbon, thereby improving the removal rate of ions. The amino-modified activated carbon can effectively adsorb negative ions, significantly improve the ability of the electrode to capture ions and the ability to shield the common ion effect, thereby significantly extending the life of the electrode. In particular, the grafting rate of the amino group of the amino-modified activated carbon is 20% to 75%. The inventor found that if the amino grafting rate of the activated carbon is too small, the amino group cannot well shield the common ion, resulting in a decrease in the number of cycles, and if the amino grafting rate of the activated carbon is too large, the excessive amino group may occupy too many intrinsic adsorption sites of the activated carbon, thereby reducing the adsorption capacity of the activated carbon for ions. In addition, too much amino group may also affect the pore structure of activated carbon, resulting in a decrease in the overall adsorption performance. The present application controls the amino grafting rate of activated carbon to between 20% and 75%, which can not only significantly improve the ion removal performance of the electrode, but also effectively improve the cycle performance of the electrode. Therefore, the positive electrode of the present application can improve the ion removal rate, and the positive electrode has a longer service life.

[0006] In addition, the capacitor deionization positive electrode according to the above embodiment of the present invention also has the following technical features: In some embodiments of the present invention, the grafting rate of amino groups of the amino-modified activated carbon is 50% to 60%.

[0007] In some embodiments of the present invention, the thickness of the positive electrode active material layer on one side of the first current collector is 30 um to 200 um.

[0008] In some embodiments of the present invention, the positive electrode active material layer further includes a first conductive agent and a first binder.

[0009] In a second aspect of the present invention, the present invention provides a capacitor deionization negative electrode. According to an embodiment of the present invention, the capacitor deionization negative electrode comprises a second current collector and a negative electrode active material layer, the negative electrode active material layer is adjacent to at least one side of the second current collector, the negative electrode active material layer comprises sulfonic acid group-modified activated carbon, and the grafting rate of the sulfonic acid group of the sulfonic acid group-modified activated carbon is 10% to 60%.

[0010] According to the above-mentioned embodiment of the present invention, the capacitor deionization negative electrode comprises a second current collector and a negative electrode active material layer, the negative electrode active material layer is adjacent to at least one side of the second current collector, and the negative electrode active material layer comprises activated carbon modified by sulfonic acid groups. The sulfonic acid group modification enriches the surface groups of the activated carbon, which can make full use of the specific surface area of ​​the activated carbon and improve the utilization rate of the activated carbon. At the same time, the sulfonic acid group modification improves the wettability of the activated carbon surface with electrolytic water, reduces the diffusion resistance of ions in the activated carbon electrode, and improves the conductivity of the activated carbon, thereby improving the ion removal rate. The activated carbon modified by the sulfonic acid group can effectively adsorb positive ions, significantly improve the ability of the electrode to capture ions and the ability to shield the common ion effect, thereby significantly extending the life of the electrode. In particular, the grafting rate of the sulfonic acid group of the sulfonic acid group-modified activated carbon is 10% to 60%. The inventors found that if the sulfonic acid group grafting rate of activated carbon is too small, too few sulfonic acid groups cannot shield the common ion effect, and the intrinsic adsorption performance of activated carbon is attenuated, resulting in a decrease in cycle performance. If the sulfonic acid group grafting rate of activated carbon is too large, it will occupy the adsorption sites of the intrinsic activated carbon, resulting in an imbalance in the performance of activated carbon, which is not conducive to improving the overall adsorption performance. The present application controls the sulfonic acid group grafting rate of activated carbon between 10% and 60%, which can not only significantly improve the ion removal performance of the electrode, but also effectively improve the cycle performance of the electrode. Therefore, the negative electrode of the present application can improve the removal rate of ions, and the negative electrode has a longer service life.

[0011] In addition, the capacitor deionization negative electrode according to the above embodiment of the present invention also has the following technical features: In some embodiments of the present invention, the grafting rate of sulfonic acid groups of the sulfonic acid group-modified activated carbon is 30% to 40%.

[0012] In some embodiments of the present invention, the thickness of the negative electrode active material layer on one side of the second current collector is 30 um to 200 um.

[0013] In some embodiments of the present invention, the negative electrode active material layer further includes a second conductive agent and a second binder.

[0014] In a third aspect of the present invention, the present invention provides a capacitor deionization device. According to an embodiment of the present invention, the capacitor deionization device includes the above-mentioned positive electrode and / or the above-mentioned negative electrode. Thus, the capacitor deionization device has an excellent ion removal rate and a long service life.

[0015] In some embodiments of the present invention, the capacitive deionization device includes the positive electrode and the negative electrode, the grafting rate of the amino group of the amino-modified activated carbon of the positive electrode is 40%~60%, and the grafting rate of the sulfonic acid group of the sulfonic acid group-modified activated carbon of the negative electrode is 20%~50%. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0017] Figure 1 Schematic diagram of the positive electrode structure of capacitor deionization according to an embodiment of the present invention; Figure 2 Schematic diagram of the negative electrode structure of capacitor deionization according to an embodiment of the present invention; Figure 3 It is a graph showing the cycle performance test results of the capacitive deionization devices of Example 3 of the present invention and Comparative Example 1. DETAILED DESCRIPTION

[0018] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the drawings of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0019] In the first aspect of the present invention, the present invention provides a capacitor deionization positive electrode. According to an embodiment of the present invention, reference Figure 1 The capacitor deionization positive electrode includes a first current collector 100 and a positive active material layer 200, wherein the positive active material layer 200 is adjacent to at least one side of the first current collector 100, and the positive active material layer 200 includes amino-modified activated carbon, wherein the grafting rate of amino groups of the amino-modified activated carbon is 20% to 75%.

[0020] According to the above embodiment of the present invention, the capacitor deionization positive electrode comprises a first current collector 100 and a positive electrode active material layer 200, the positive electrode active material layer 200 is adjacent to at least one side of the first current collector 100, and the positive electrode active material layer 200 comprises amino-modified activated carbon, and the grafting rate of amino groups of the amino-modified activated carbon is 20% to 75%. For example, the grafting rate of amino groups is 20%, 30%, 40%, 50%, 60%, 70%, 75%, etc., and the grafting rate is greater than or equal to 20%, 30%, 40%, etc., and less than or equal to 50%, 60%, 70%, 75%, etc. Amino modification enriches the surface groups of activated carbon, can make full use of the specific surface area of ​​activated carbon, and improve the utilization rate of activated carbon. At the same time, the modification of amino groups improves the wettability of the activated carbon surface with electrolytic water, reduces the diffusion resistance of ions in the activated carbon electrode, and improves the conductivity of activated carbon, thereby improving the removal rate of ions. Activated carbon modified with amino groups can effectively adsorb negative ions, significantly improve the ability of the electrode to capture ions and shield the common ion effect, thereby significantly extending the life of the electrode. In particular, the inventors found that if the amino grafting rate of the activated carbon is too small, the amino group cannot well shield the common ion, resulting in a decrease in the number of cycles. If the amino grafting rate of the activated carbon is too large, the excessive amino group may occupy too many intrinsic adsorption sites of the activated carbon, thereby reducing the adsorption capacity of the activated carbon for ions. In addition, too many amino groups may also affect the pore structure of the activated carbon, resulting in a decrease in the overall adsorption performance. The present application controls the amino grafting rate of the activated carbon between 20% and 75%, which can not only significantly improve the ion removal performance of the electrode, but also effectively improve the cycle performance of the electrode. Therefore, the positive electrode of the present application can improve the removal rate of ions, and the positive electrode has a longer service life.

[0021] The first current collector is a conventional component in the art, and those skilled in the art may select it according to actual conditions. For example, the first current collector includes but is not limited to copper foil, aluminum foil, stainless steel foil, titanium foil, nickel foil, etc.

[0022] It should be noted that the grafting rate of amino groups: the grafting rate of amino groups on the surface of activated carbon is calculated by acid-base titration test and difference method. 1. The content of alkali V1 and V2 on the surface of activated carbon before and after grafting is tested by acid-base titration method; 2. Grafting rate = (1-V1 / V2) * 100% to calculate the grafting rate.

[0023] Preferably, the grafting rate of the amino group of the amino-modified activated carbon is 50% to 60%.

[0024] According to an embodiment of the present invention, the thickness of the positive electrode active material layer on one side of the first current collector is 30um~200um. For example, the thickness is greater than or equal to 30um, 50um, 80um, etc., and less than or equal to 90um, 130um, 160um, 200um, etc. The inventors found that controlling the thickness of the positive electrode active material layer on one side of the first current collector within the range of 30um~200um can ensure a certain adsorption amount of the positive electrode active material layer, and the adsorption performance is good. At the same time, the adhesion between the positive electrode active material layer and the current collector is ensured, the resistance is reduced, cracking is avoided, and the service life is extended.

[0025] According to an embodiment of the present invention, the positive electrode active material layer further includes a first conductive agent and a first binder.

[0026] According to an embodiment of the present invention, based on the total mass of the positive electrode active material layer, the mass proportion of the first conductive agent is 4% to 8%, for example, greater than or equal to 4%, 4.5%, 5%, etc., and less than or equal to 6%, 7%, 8%, etc.

[0027] According to an embodiment of the present invention, the first conductive agent includes but is not limited to acetylene black, conductive carbon black, and graphite powder.

[0028] According to an embodiment of the present invention, based on the total mass of the positive electrode active material layer, the mass proportion of the first binder is 5% to 10%, for example, greater than or equal to 5%, 6%, 7%, etc., and less than or equal to 8%, 9%, 10%, etc.

[0029] According to an embodiment of the present invention, the first adhesive includes but is not limited to polyurethane, polystyrene, polyacrylate, and polytetrafluoroethylene.

[0030] In a second aspect of the present invention, the present invention provides a capacitor deionization negative electrode. According to an embodiment of the present invention, reference Figure 2 The capacitor deionization negative electrode includes a second current collector 300 and a negative electrode active material layer 400, wherein the negative electrode active material layer 400 is adjacent to at least one side of the second current collector 300, and the negative electrode active material layer 400 includes sulfonic acid group-modified activated carbon, and the grafting rate of the sulfonic acid group of the sulfonic acid group-modified activated carbon is 10% to 60%.

[0031] According to the above embodiment of the present invention, the capacitor deionization negative electrode comprises a second current collector 300 and a negative electrode active material layer 400, wherein the negative electrode active material layer 400 is adjacent to at least one side of the second current collector 300, and the negative electrode active material layer 400 comprises activated carbon modified by sulfonic acid groups, wherein the grafting rate of the sulfonic acid groups of the activated carbon modified by sulfonic acid groups is 10% to 60%. For example, the grafting rate of the sulfonic acid groups is 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, etc., and the grafting rate is greater than or equal to 10%, 15%, 20%, 25%, etc., and less than or equal to 30%, 35%, 40%, 45%, 50%, 55%, 60%, etc. Sulfonic acid group modification enriches the surface groups of activated carbon, which can make full use of the specific surface area of ​​activated carbon and improve the utilization rate of activated carbon. At the same time, the modification of sulfonic acid group improves the wettability of activated carbon surface and electrolytic water, reduces the diffusion resistance of ions in activated carbon electrode, improves the conductivity of activated carbon, and thus improves the removal rate of ions. Activated carbon modified by sulfonic acid group can effectively adsorb positive ions, significantly improve the ability of electrode to capture ions and shield the common ion effect, thereby significantly extending the life of the electrode. In particular, the inventor found that if the sulfonic acid group grafting rate of activated carbon is too small, too few sulfonic acid groups cannot shield the common ion effect, and the intrinsic adsorption performance of activated carbon is attenuated, resulting in a decrease in cycle performance. If the sulfonic acid group grafting rate of activated carbon is too large, it will occupy the adsorption sites of intrinsic activated carbon, resulting in an imbalance in the performance of activated carbon, which is not conducive to improving the overall adsorption performance. The present application controls the sulfonic acid group grafting rate of activated carbon between 10% and 60%, which can not only significantly improve the ion removal performance of the electrode, but also effectively improve the cycle performance of the electrode. Therefore, by using the negative electrode of the present application, the ion removal rate can be improved, and the negative electrode has a longer service life.

[0032] It should be noted that the grafting rate of sulfonic acid groups: The grafting rate of sulfonic acid groups on the surface of activated carbon is calculated using Fourier transform infrared spectroscopy and area difference method. 1. Use Fourier transform infrared spectroscopy to test the infrared spectra of the surface groups of activated carbon before and after grafting. 2. Compare the characteristic absorption peak of the sulfonic acid group, and compare the area (S) change of the characteristic absorption peak of the sulfonic acid group before and after grafting. Use the grafting rate = (1-S before / S after) * 100% to get the size of the grafting rate.

[0033] The second current collector is a conventional component in the art, and those skilled in the art may select it according to actual conditions. For example, the second current collector includes but is not limited to copper foil, aluminum foil, stainless steel foil, titanium foil, nickel foil, etc.

[0034] Preferably, the grafting rate of sulfonic acid groups of the sulfonic acid group-modified activated carbon is 30% to 40%.

[0035] According to an embodiment of the present invention, the thickness of the negative electrode active material layer on one side of the second current collector is 30um~200um. For example, the thickness is greater than or equal to 30um, 50um, 80um, etc., and less than or equal to 90um, 130um, 160um, 200um, etc. The inventors found that controlling the thickness of the negative electrode active material layer on one side of the second current collector within the range of 30um~200um can ensure a certain adsorption amount of the negative electrode active material layer, and the adsorption performance is good. At the same time, the adhesion between the negative electrode active material layer and the current collector is ensured, the resistance is reduced, cracking is avoided, and the service life is extended.

[0036] According to an embodiment of the present invention, the negative electrode active material layer further includes a second conductive agent and a second binder.

[0037] According to an embodiment of the present invention, based on the total mass of the negative electrode active material layer, the mass proportion of the second conductive agent is 4% to 8%, for example, the mass proportion is greater than or equal to 4%, 4.5%, 5%, etc., and less than or equal to 5.5%, 6%, 6.5%, 7%, 8%, etc.

[0038] According to an embodiment of the present invention, the second conductive agent includes but is not limited to acetylene black, conductive carbon black, and graphite powder.

[0039] According to an embodiment of the present invention, based on the total mass of the negative electrode active material layer, the mass proportion of the second binder is 5% to 10%, for example, greater than or equal to 5%, 6%, 7%, etc., and less than or equal to 8%, 9%, 10%, etc.

[0040] According to an embodiment of the present invention, the second binder includes but is not limited to polyurethane, polystyrene, polyacrylate, and polytetrafluoroethylene.

[0041] In the third aspect of the present invention, the present invention provides a capacitor deionization device. According to an embodiment of the present invention, the capacitor deionization device includes the above-mentioned positive electrode and / or the above-mentioned negative electrode. As a result, the capacitor deionization device has an excellent ion removal rate and a long service life. It should be noted that the features and advantages described above for the positive electrode and the negative electrode are also applicable to the capacitor deionization device.

[0042] Preferably, the capacitor deionization device includes the above-mentioned positive electrode and the above-mentioned negative electrode. The inventors found that the capacitor deionization device includes the above-mentioned positive electrode and the above-mentioned negative electrode at the same time, and the combination of sulfonic acid group and amino group grafting has a synergistic effect. In adsorption, the electrodes as positive and negative electrodes respectively adsorb anions and cations. The ungrafted activated carbon only relies on the driving force of the electric field to capture ions in the pore size of the activated carbon. The activated carbon grafted with sulfonic acid groups has the function of automatically capturing cations. Combined with the driving force of the electric field, the overall ability to capture cations is stronger; the corresponding activated carbon grafted with amino groups can automatically capture anions, and combined with the electric field, better capture anions. The combination of sulfonic acid group and amino group grafting significantly improves the adsorption capacity of ions, thereby significantly improving the adsorption performance of the electrode.

[0043] According to an embodiment of the present invention, the capacitive deionization device includes the positive electrode and the negative electrode, the grafting rate of the amino group of the amino-modified activated carbon of the positive electrode is 40% to 60%, and the grafting rate of the sulfonic acid group of the sulfonic acid group-modified activated carbon of the negative electrode is 20% to 50%. The inventors have found that if the capacitive deionization device includes a positive electrode and a negative electrode, controlling the grafting rate of the amino group of the activated carbon and the grafting rate of the sulfonic acid group of the activated carbon within the above range can significantly improve the ion removal rate and cycle life of the device.

[0044] If no specific techniques or conditions are specified in the examples, the techniques or conditions described in the literature in the field or the product instructions are used. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be purchased through regular channels.

[0045] Example 1

[0046] (1) Preparation of capacitor deionization positive electrode

[0047] (a) 9 mol / L nitric acid solution was added to activated carbon, wherein the molar ratio of activated carbon to nitric acid was 1:40, and the mixture was stirred at 70°C for 10 h. The mixture was vacuum filtered, washed with distilled water until neutral, and dried at 110°C for 10 h to surface treat the activated carbon, thereby obtaining surface-treated activated carbon.

[0048] (b) Take out 200 mg of the dried surface-treated activated carbon, add 6 g of thionyl chloride, reflux at 78°C for 4 h, evaporate the remaining thionyl chloride under reduced pressure to obtain chlorinated activated carbon, then slowly pour it into 6 g of ethylenediamine, react at 120°C for 10 h, vacuum filter and wash with distilled water until neutral, dry at 110°C for 6 h to obtain amino group-grafted activated carbon (amino-modified activated carbon). The amino grafting rate was tested to be 58%.

[0049] (c) Weigh the corresponding masses with a mass ratio of amino-modified activated carbon: conductive carbon black: binder = 88:5:7 and mix the powders. After mixing, add the solid powders into the solvent to form a 30% solid content solution, stir it with a stirrer for 4 hours to form a uniform slurry, and then use a scraper to apply it to the current collector, dry it at 80°C for 4 hours, and roll it with a roller press 90T to form a positive electrode with a single-sided coating thickness of 85um.

[0050] (2) Preparation of capacitor deionization negative electrode

[0051] Weigh the corresponding mass with a mass ratio of pure activated carbon: conductive carbon black: binder = 88:5:7 and mix the powders. After mixing, add the solid powder to the solvent to form a 30% solid content solution. Use a stirrer to stir for 4 hours to form a uniform slurry. Use a scraper to apply it to the current collector, dry it at 80°C for 4 hours, and use a roller press 90T to form a negative electrode with a single-sided coating thickness of 85um.

[0052] (3) Preparation of capacitive deionization devices

[0053] The positive electrode-separator-negative electrode-separator are arranged alternately to prepare a rolled capacitor deionization device.

[0054] Example 2

[0055] (1) Preparation of capacitor deionization positive electrode

[0056] The corresponding mass was weighed and powdered in a mass ratio of pure activated carbon: conductive carbon black: binder = 88:5:7. After mixing, the solid powder was added to the solvent to form a 30% solid content solution. The slurry was stirred for 4 hours using a stirrer to form a uniform slurry. The slurry was then applied to the current collector using a scraper coating device, dried at 80°C for 4 hours, and rolled using a 90T roller press to form a positive electrode with a single-sided coating thickness of 85um.

[0057] (2) Preparation of capacitor deionization negative electrode

[0058] (a) 5.54 g of anhydrous p-aminobenzenesulfonic acid was added to 150 mL of concentrated sulfuric acid and stirred at room temperature until no obvious particles were present, and then 2.21 g of sodium nitrite was added and reacted in a 10-15°C water bath for 20 min. Then 200 mg of surface-treated activated carbon (same as in Example 1) and 1.2 g of azobisisobutyronitrile were added and reacted in a 40°C water bath for 6 h. Finally, the suspension was poured into distilled water containing ice cubes and filtered and washed until neutral. Then, the suspension was washed and filtered with acetone and dimethylformamide, and vacuum dried at 80°C for 24 h to obtain sulfonic acid grafted activated carbon (sulfonic acid modified activated carbon). The grafting rate of sulfonic acid groups was tested to be 35%.

[0059] (b) Weigh the corresponding masses of sulfonic acid modified activated carbon: conductive carbon black: binder in a mass ratio of 88:5:7 and mix the powders. After mixing, add the solid powders into a solvent to form a 30% solid content solution. Stir the solution for 4 hours using a stirrer to form a uniform slurry. Then use a scraper to apply the slurry to the current collector, dry it at 80°C for 4 hours, and press it using a roller press at 90T to form a negative electrode with a single-sided coating thickness of 85um.

[0060] (3) Preparation of capacitive deionization devices

[0061] The preparation process of the capacitive deionization device is the same as that of Example 1.

[0062] Example 3

[0063] (1) Preparation of capacitor deionization positive electrode

[0064] The preparation process of the capacitor deionization positive electrode is the same as that in Example 1.

[0065] (2) Preparation of capacitor deionization negative electrode

[0066] The preparation process of the capacitor deionization negative electrode is the same as that of Example 2.

[0067] (3) Preparation of capacitive deionization devices

[0068] The preparation process of the capacitive deionization device is the same as that of Example 1.

[0069] Example 4

[0070] (1) Preparation of capacitor deionization positive electrode

[0071] (a) 100 mg of dried surface-treated activated carbon (the same as in Example 1) was taken out, 6 g of thionyl chloride was added, and the mixture was refluxed at 78° C. for 4 h. After the remaining thionyl chloride was distilled off under reduced pressure, chlorinated activated carbon was obtained, which was then slowly poured into 6 g of ethylenediamine, reacted at 120° C. for 10 h, vacuum filtered, washed with distilled water until neutral, and dried at 110° C. for 6 h to obtain amino group-grafted activated carbon. The amino group grafting rate was tested to be 28%.

[0072] (b) Weigh the corresponding masses with a mass ratio of amino-modified activated carbon: conductive carbon black: binder = 88:5:7 and mix the powders. After mixing, add the solid powders into the solvent to form a 30% solid content solution, stir it with a stirrer for 4 hours to form a uniform slurry, and then use a scraper to apply it to the current collector, dry it at 80°C for 4 hours, and roll it with a roller press 90T to form a positive electrode with a single-sided coating thickness of 85um.

[0073] (2) Preparation of capacitor deionization negative electrode

[0074] (a) 5.54 g of anhydrous p-aminobenzenesulfonic acid was added to 150 mL of concentrated sulfuric acid and stirred at room temperature until no obvious particles were present, and then 2.21 g of sodium nitrite was added and reacted in a 10-15°C water bath for 20 min. Then 500 mg of surface-treated activated carbon (same as in Example 1) and 1.2 g of azobisisobutyronitrile were added and reacted in a 40°C water bath for 6 h. Finally, the suspension was poured into distilled water containing ice cubes and filtered and washed until neutral. Then, it was continuously washed and filtered with acetone and dimethylformamide, and vacuum dried at 80°C for 24 h to obtain sulfonic acid grafted activated carbon. The grafting rate of the sulfonic acid group was tested to be 15%.

[0075] (b) Weigh the corresponding masses of sulfonic acid modified activated carbon: conductive carbon black: binder in a mass ratio of 88:5:7 and mix the powders. After mixing, add the solid powders into a solvent to form a 30% solid content solution. Stir the solution for 4 hours using a stirrer to form a uniform slurry. Then use a scraper to apply the slurry to the current collector, dry it at 80°C for 4 hours, and press it using a roller press at 90T to form a negative electrode with a single-sided coating thickness of 85um.

[0076] (3) Preparation of capacitive deionization devices

[0077] The preparation process of the capacitive deionization device is the same as that of Example 1.

[0078] Example 5

[0079] (1) Preparation of capacitor deionization positive electrode

[0080] The main difference between the capacitor deionization positive electrode of Example 5 and Example 4 is that the amino grafting rate of the activated carbon used in Example 5 is 25%.

[0081] (2) Preparation of capacitor deionization negative electrode

[0082] The main difference between the capacitor deionization negative electrode of Example 5 and Example 4 is that the sulfonic acid group grafting rate of the activated carbon used in Example 5 is 55%.

[0083] (3) Preparation of capacitive deionization devices

[0084] The preparation process of the capacitive deionization device is the same as that of Example 1.

[0085] Comparative Example 1

[0086] (1) Preparation of capacitor deionization positive electrode

[0087] The corresponding mass was weighed and powdered in a mass ratio of pure activated carbon: conductive carbon black: binder = 88:5:7. After mixing, the solid powder was added to the solvent to form a 30% solid content solution. The slurry was stirred for 4 hours using a stirrer to form a uniform slurry. The slurry was then applied to the current collector using a scraper coating device, dried at 80°C for 4 hours, and rolled using a 90T roller press to form a positive electrode with a single-sided coating thickness of 85um.

[0088] (2) Preparation of capacitor deionization negative electrode

[0089] Weigh the corresponding mass with a mass ratio of pure activated carbon: conductive carbon black: binder = 88:5:7 and mix the powders. After mixing, add the solid powder to the solvent to form a 30% solid content solution. Use a stirrer to stir for 4 hours to form a uniform slurry. Use a scraper to apply it to the current collector, dry it at 80°C for 4 hours, and use a roller press 90T to form a negative electrode with a single-sided coating thickness of 85um.

[0090] (3) Preparation of capacitive deionization devices

[0091] The preparation process of the capacitive deionization device is the same as that of Example 1.

[0092] Comparative Example 2

[0093] (1) Preparation of capacitor deionization positive electrode

[0094] The main difference between the capacitor deionization positive electrode of Comparative Example 2 and Example 4 is that the amino grafting rate of the activated carbon used in Comparative Example 2 is 80%.

[0095] (2) Preparation of capacitor deionization negative electrode

[0096] The main difference between the capacitor deionization negative electrode of Comparative Example 2 and Example 4 is that the sulfonic acid group grafting rate of the activated carbon used in Comparative Example 2 is 70%.

[0097] (3) Preparation of capacitive deionization devices

[0098] The preparation process of the capacitive deionization device is the same as that of Example 1.

[0099] Comparative Example 3

[0100] (1) Preparation of capacitor deionization positive electrode

[0101] The main difference between the capacitor deionization positive electrode of Comparative Example 3 and Example 4 is that the amino grafting rate of the activated carbon used in Comparative Example 3 is 15%.

[0102] (2) Preparation of capacitor deionization negative electrode

[0103] The main difference between the capacitor deionization negative electrode of Comparative Example 3 and Example 4 is that the sulfonic acid group grafting rate of the activated carbon used in Comparative Example 3 is 5%.

[0104] (3) Preparation of capacitive deionization devices

[0105] The preparation process of the capacitive deionization device is the same as that of Example 1.

[0106] The performance of the capacitive deionization devices prepared in Examples 1-5 and Comparative Examples 1-3 was measured, and the specific method was as follows: Ion removal rate (%): Raw water containing sodium chloride, sodium bicarbonate, calcium chloride and magnesium sulfate is prepared in a certain proportion. The water quality of the raw water at this time is recorded as TDS1. It is passed into the capacitive deionization device at a flow rate of 1L / min / m2. The water quality of the effluent is recorded as TDS2. The ion removal rate = (1-TDS2 / TDS1) * 100%.

[0107] Cycle life: The number of cycles is recorded when the ion removal rate decays to 50% of the initial value.

[0108] The test results of the performance of the capacitive deionization devices prepared in Examples 1-5 and Comparative Examples 1-3 are shown in Table 1.

[0109] Table 1

[0110] Combination Figure 3 ,As can be seen from Table 1, grafting a certain amount of sulfonic ,acid groups and amino groups on activated carbon can ,on one hand, improve the overall adsorption performance and on the other hand, also prolong its cycle life.

[0111] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A capacitor deionization positive electrode, It is characterized in that The invention comprises a first current collector and a positive electrode active material layer, wherein the positive electrode active material layer is adjacent to at least one side of the first current collector, and the positive electrode active material layer comprises amino-modified activated carbon, wherein the grafting rate of amino groups of the amino-modified activated carbon is 20% to 75%.

2. The positive electrode according to claim 1, It is characterized in that The grafting rate of amino groups of the amino-modified activated carbon is 50% to 60%.

3. The positive electrode according to claim 1, It is characterized in that The thickness of the positive electrode active material layer on one side of the first current collector is 30 um to 200 um.

4. The positive electrode according to any one of claims 1 to 3, It is characterized in that The positive electrode active material layer further includes a first conductive agent and a first binder.

5. A capacitor deionization negative electrode, It is characterized in that The invention comprises a second current collector and a negative electrode active material layer, wherein the negative electrode active material layer is adjacent to at least one side of the second current collector, and the negative electrode active material layer comprises activated carbon modified by sulfonic acid groups, wherein the grafting rate of sulfonic acid groups of the activated carbon modified by sulfonic acid groups is 10% to 60%.

6. The negative electrode according to claim 5, It is characterized in that The grafting rate of the sulfonic acid group of the sulfonic acid group-modified activated carbon is 30% to 40%.

7. The negative electrode according to claim 5, It is characterized in that The thickness of the negative electrode active material layer on one side of the second current collector is 30 um to 200 um.

8. The negative electrode according to any one of claims 5 to 7, It is characterized in that The negative electrode active material layer further includes a second conductive agent and a second binder.

9. A capacitive deionization device, It is characterized in that It comprises the positive electrode according to any one of claims 1 to 4 and / or the negative electrode according to any one of claims 5 to 8.

10. The capacitive deionization device according to claim 9, It is characterized in that The capacitive deionization device comprises the positive electrode and the negative electrode, the grafting rate of amino groups of the amino-modified activated carbon of the positive electrode is 40% to 60%, and the grafting rate of sulfonic acid groups of the sulfonic acid-modified activated carbon of the negative electrode is 20% to 50%.

Citation Information

Patent Citations

  • Functional mesoporous carbon electrode material and preparation method thereof

    CN109133276A

  • Flowing electrode, application and regeneration method thereof, and method for enriching uranium in uranium-containing water body by using flowing electrode capacitive deionization device

    CN117383666A

  • Electrode for capacitive deionization device, method of manufacturing the electrode, and capacitive deionization device having the electrode

    US20090020430A1

Cited By

  • Electrode for capacitive deionization and preparation method thereof

    CN119528283A