Secondary sintered microcrystalline ceramic glaze, preparation method thereof and microcrystalline ceramic glaze brick
The microcrystals synthesized by solid-phase reaction method are formed through the secondary sintering method, which solves the problems of narrow firing range and poor stability of microcrystalline ceramic glaze, and improves the stability and adaptability of glaze and roughness, reducing the stability and adaptability of glaze. production difficulty and cost.
Patent Information
- Application Number
- CN202410973669.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-07-19
AI Technical Summary
The existing microcrystalline ceramic glaze has a narrow firing range and poor production stability, resulting in the glaze, transparency and surface roughness that are easily affected by kiln temperature fluctuations, and the formulation debugging is difficult.
The microcrystalline ceramic glaze preparation method is adopted to obtain the sintered material by ball milling and calcining the prescribed raw material formula, mixed and grinding into glaze slurry, and secondary calcining is carried out at a specific temperature to form microcrystals synthesized by solid phase reaction method. Broaden the firing temperature range and reduce pinhole bubbles and gloss changes.
The gloss gloss of the gloss as low as 10 degrees and the surface roughness as low as 0.6 microns are achieved, and the stability is improved. The glaze effect is less affected by the kiln temperature and thickness, and the formulation adaptability is enhanced, reducing production difficulty and cost.
Smart Images

Figure CN118878211A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building ceramics, and in particular to a secondary sintered microcrystalline ceramic glaze and a preparation method thereof, and a microcrystalline ceramic glaze brick. Background Art
[0002] The microcrystalline ceramic glaze used for ceramic tiles is formulated, water and additives are added, ground into a glaze slurry below 325 mesh, and glazed and fired, which can also be called the powder sintering method. There are usually two formula structures. One is to use a full raw material formula. This formula requires a higher kiln temperature and a longer high-fire insulation time than the current ceramic tile industry to burn out the microcrystalline ceramic glaze with a smooth glaze surface and low gloss. This does not meet the needs of low-carbon production and is generally not adopted. The second is to use a semi-raw material formula. At present, the ceramic industry produces microcrystalline ceramic glaze products with this formula structure, that is, kaolin, feldspar, quartz, calcite, burned talc, barium carbonate, strontium carbonate, etc., plus 1 to 3 kinds of glass powder (commonly known as frit in the ceramic industry) and other firing.
[0003] However, during the production process of the semi-raw material structured microcrystalline ceramic glaze, the firing range of the glaze is narrow. When the kiln temperature fluctuates slightly, the gloss, transparency and surface roughness of the glaze surface are very likely to change. Therefore, the production stability is poor.
[0004] Therefore, the prior art has defects and needs to be improved and developed. Summary of the invention
[0005] The technical problem to be solved by the present invention is that, in view of the above-mentioned defects of the prior art, a secondary sintered microcrystalline ceramic glaze and a preparation method thereof, as well as microcrystalline ceramic glaze bricks are provided, aiming to solve the problems of narrow firing range and poor production stability of the microcrystalline ceramic glaze with a semi-raw material structure in the prior art during the production process.
[0006] The technical solution adopted by the present invention to solve the technical problem is as follows:
[0007] The first aspect of the present application provides a method for preparing a twice-sintered microcrystalline ceramic glaze, wherein the method comprises:
[0008] After mixing the raw materials according to the predetermined formula, ball milling is performed to obtain glaze powder;
[0009] calcining the glaze powder material to obtain a sintered material;
[0010] Mixing ingredients according to a predetermined microcrystalline ceramic glaze formula and grinding them into glaze slurry, wherein the microcrystalline ceramic glaze formula includes the sintering material;
[0011] The glaze slurry is applied to the brick and then secondary calcined to obtain a microcrystalline ceramic glaze.
[0012] In one embodiment of the present application, the raw material formula includes a first raw material formula and a second raw material formula, and the first raw material formula includes, by weight percentage:
[0013] Kaolin 10-15%, potassium feldspar 18-25%, frit 5-10%, barium carbonate 10-13%, calcite 18-30%, zinc oxide 4-8%, quartz 18-25%;
[0014] The second raw material formula, measured by weight percentage, includes:
[0015] Potassium feldspar 45-55%, frit 6-10%, barium carbonate 10-18%, calcite 20-25%, zinc oxide 3-6%, quartz 12-18%.
[0016] In one embodiment of the present application, the chemical components of the frit include, by weight percentage:
[0017] Loss on ignition 0.3-1.2%, SiO2 50-60%, Al2O3 8-12%, Fe2O3 0.1-0.5%, TiO20.08-0.2%, CaO 16-20%, MgO 5-8%, K2O 3.5-5%, Na2O 2-3%, ZnO 0.3-0.6%, B2O3 0.1-0.3%, BaO 0.6-1.5%.
[0018] In one embodiment of the present application, the process of preparing the raw materials according to a predetermined raw material formula and then ball milling to obtain the glaze powder material comprises:
[0019] After mixing the ingredients according to the predetermined raw material formula, sodium carboxymethyl cellulose, sodium tripolyphosphate and water are added for wet ball milling to a fineness of 0.1-0.3% of the residue on a 325-mesh sieve, and then spray-dried to obtain a glaze powder;
[0020] Alternatively, the raw materials are mixed according to a predetermined formula and then conveyed to a Raymond mill for fine grinding to a fineness of 0.1-0.3% of the residue on a 325-mesh sieve to obtain a glaze powder.
[0021] In one embodiment of the present application, the glaze powder is calcined to obtain a sintered material, comprising:
[0022] The glaze powder material is calcined at a temperature of 1000-1150° C. to obtain a sintered material.
[0023] In one embodiment of the present application, the microcrystalline ceramic glaze formula comprises, by weight percentage:
[0024] 8-12% kaolin, 60-90% sintering material, 0-5% ultrafine corundum powder, 0-5% ultrafine alumina powder, 0-8% calcined kaolin, 0-30% potassium feldspar, 0-20% sodium feldspar, 0-5% wollastonite, 0-8% burned talc, 0-10% dolomite, 0-12% calcite, 0-8% barium carbonate, 0-5% strontium carbonate, and 0-8% zinc oxide.
[0025] In one embodiment of the present application, the glaze slurry is applied to a brick and then subjected to secondary calcination to obtain a microcrystalline ceramic glaze, comprising:
[0026] After the glaze slurry is applied to the brick, secondary calcination is performed at a temperature of 1140-1230° C. to obtain a microcrystalline ceramic glaze.
[0027] In one embodiment of the present application, the glaze slurry is applied to a brick and then subjected to secondary calcination to obtain a microcrystalline ceramic glaze, comprising:
[0028] If the glaze slurry is prepared from the sintered material prepared from the first raw material formula, the glaze slurry is applied to the brick blank and then secondary calcined at a temperature of 1190° C. to 1230° C. to obtain a microcrystalline ceramic glaze;
[0029] If the glaze slurry is prepared from a sintered material prepared from the second raw material formula, the glaze slurry is applied to the brick and then secondary calcined at a temperature of 1140° C. to 1170° C. to obtain a microcrystalline ceramic glaze.
[0030] A second aspect of the present application provides a microcrystalline ceramic glaze, wherein the microcrystalline ceramic glaze is prepared based on the preparation method of the secondary sintered microcrystalline ceramic glaze as described above.
[0031] The third aspect of the present application provides a microcrystalline ceramic glazed tile, wherein the microcrystalline ceramic glaze as described above is applied on the microcrystalline ceramic glaze tile.
[0032] The present invention discloses a microcrystalline ceramic glaze with secondary sintering and a preparation method thereof, and a microcrystalline ceramic glaze brick, the method comprising: mixing ingredients according to a predetermined raw material formula and then ball milling to obtain a glaze powder; calcining the glaze powder to obtain a sintering material; mixing ingredients according to a predetermined microcrystalline ceramic glaze formula and grinding into a glaze slurry, wherein the microcrystalline ceramic glaze formula includes the sintering material; applying the glaze slurry to a brick blank and then calcining it for the secondary time to obtain a microcrystalline ceramic glaze. The microcrystals in the microcrystalline ceramic glaze prepared by the present invention are formed during the first sintering, and will not be completely melted during the secondary sintering, and do not need to go through a process of first melting and then crystallization, therefore, the influence of the kiln temperature is minimal, the firing range is wide, and it is conducive to the stability of production. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1The present invention is a flowchart of a preferred embodiment of a method for preparing a secondary sintered microcrystalline ceramic glaze.
[0034] Figure 2 It is the diffraction spectrum of the sintering material obtained by the first raw material formula in the present invention. DETAILED DESCRIPTION
[0035] In order to make the purpose, technical solution and advantages of the present invention clearer and more specific, the present invention is further described in detail below with reference to the accompanying drawings and examples. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0036] Traditional ceramic crystal glazes can be divided into giant crystal glazes, fine crystal glazes and microcrystalline ceramic glazes according to the size of the crystals in the glaze. Zinc and titanium crystal glazes have large crystals and belong to giant crystal glazes; tea-leaf and gold dust glazes have special crystal effects visible to the naked eye, and the crystal shape can be seen under a magnifying glass of about 10 times, which belongs to fine crystal glazes; while microcrystalline ceramic glazes cannot be seen by the naked eye and need to be specially treated and observed under a microscope.
[0037] The crystals in the crystalline glaze are all precipitated from the melt. There are two types of technical means. One is to melt the formula material at high temperature, shape it after cooling or before cooling, and then perform low-temperature heat treatment to precipitate crystals. This is the manufacturing process of microcrystalline glass. The other is to apply the formula material to the surface of the formed body, melt it at high temperature during firing, and crystallize it during cooling. Famous glazes of traditional ceramics such as zinc crystal glaze, iron red glaze, tea dust, gold sand glaze, etc. all belong to this category.
[0038] The existing preparation processes of microcrystalline glass for architectural decoration can be divided into two types, namely sintering method and melting method. Both methods are to mix ingredients according to the formula, melt them into glass in the glass melting pool and then crystallize them. The process features are as follows:
[0039] Table 1 Classification of glass-ceramic manufacturing processes
[0040]
[0041] In the sintering production of microcrystalline glass, the sintering method can be divided into glass particle sintering method and glass powder sintering method. However, in the field of preparing microcrystalline glass for architectural decoration, the glass powder sintering method has not been actually applied. In the microcrystalline glass industry, the sintering method refers to the glass particle sintering method.
[0042] Table 2 Chemical composition requirements of mother glass for different production processes of glass-ceramics
[0043]
[0044] Among them, the specific basic chemical composition should be determined according to the selected mother glass system.
[0045] However, the microcrystalline preparation process of microcrystalline glass is not suitable for the glaze of ceramic tiles.
[0046] The microcrystalline ceramic glaze used for ceramic tiles is formulated, water and additives are added, ground into a glaze slurry below 325 mesh, and glazed and fired, which can also be called the powder sintering method. There are usually two formula structures. One is to use a full raw material formula. This formula requires a higher kiln temperature and a longer high-fire insulation time than the current ceramic tile industry to burn out the microcrystalline ceramic glaze with a smooth glaze surface and low gloss. This does not meet the needs of low-carbon production and is generally not adopted. The second is to use a semi-raw material formula. At present, the ceramic industry produces microcrystalline ceramic glaze products with this formula structure, that is, kaolin, feldspar, quartz, calcite, burned talc, barium carbonate, strontium carbonate, etc., plus 1 to 3 kinds of glass powder (commonly known as frit in the ceramic industry) and other firing.
[0047] There are many problems in the production process of semi-raw material structured microcrystalline ceramic glaze:
[0048] First, the firing range of the glaze is narrow, and fluctuations in kiln temperature within 5°C will cause changes in the glaze texture. During the production process, when the kiln temperature fluctuates slightly, the glaze surface is very likely to change in gloss, transparency, and surface roughness. The two popular microcrystalline ceramic glaze products with 12±2 degree gloss and 18±2 degree gloss have this situation. Generally, when the kiln temperature rises, the glaze gloss increases, and the transparency remains unchanged or increases; when the kiln temperature decreases, the glaze gloss decreases and the transparency decreases. This formula characteristic is a stumbling block to stable product quality.
[0049] Second, the glaze formula has poor adaptability and has high requirements for kilns. When using semi-raw glaze to produce microcrystalline ceramic glaze products, due to the differences in kiln firing conditions, the selection of frit is very critical, and a special kiln and special formula are required. Due to poor matching of frits, a common problem is that it is difficult to achieve both smooth glaze and no pinhole bubbles. If this formula system meets the conditions for smooth glaze, pinhole bubbles and other glaze defects are prone to occur; when the formula is adjusted to have no pinhole bubbles in the glaze, either the glaze is wrinkled and difficult to smooth, or the glaze is smooth but the gloss is too high, and the low gloss condition cannot be achieved.
[0050] Third, formula debugging is not easy to master, and the production cycle is often disrupted because the glaze texture fails to meet the standard. The semi-raw material microcrystalline ceramic glaze formula melts at high temperature, and the melt precipitates crystals on the glaze surface during supercooling. On the thermal analysis diagram of the formula, there are obvious endothermic peaks (the glaze melts after absorbing a lot of heat) and exothermic peaks (the melt precipitates crystals and releases heat during supercooling).
[0051] Therefore, there are many problems in producing microcrystalline ceramic glaze ceramic tiles under medium temperature fast firing conditions. The most important one is that the microcrystals in the glaze need to be precipitated from the melt under slow temperature reduction firing conditions. For semi-raw material formulas, no matter how the introduced frit formula is adjusted, it is always very difficult to crystallize from the melt under fast firing conditions. The fluctuation of kiln temperature causes the change of crystallization amount, and the change of crystallization amount leads to the change of glaze diffuse reflection, and finally leads to the change of glaze gloss, which in turn leads to a long formula debugging cycle.
[0052] The present invention provides a secondary sintered microcrystalline ceramic glaze, in which microcrystals synthesized by a solid phase reaction method are introduced into the glaze. When producing the microcrystalline ceramic glaze, the initial melting temperature of the glaze can be greatly increased, the firing temperature range of the microcrystalline ceramic glaze can be widened, pinhole bubbles in the glaze can be eliminated, the difficulty of formula debugging can be reduced, the difficulty of product production can be reduced, and the product quality rate can be improved. The problem that the glaze effect is greatly affected by the kiln temperature and the thickness of the glaze layer, the glaze has pinhole rashes, the adaptability of the glaze formula is poor, and the firing range is narrow can be solved. Under the condition of medium-temperature fast firing, the glaze gloss can be as low as below 10 degrees and the surface roughness can be as low as 0.6 microns.
[0053] The first aspect of the present application provides a method for preparing a secondary sintered microcrystalline ceramic glaze, such as Figure 1 As shown, the preparation method of the secondary sintered microcrystalline ceramic glaze includes:
[0054] Step S100: mixing raw materials according to a predetermined raw material formula and then ball milling to obtain glaze powder.
[0055] In the embodiment of the present application, the raw material formula includes a first raw material formula and a second raw material formula, and the first raw material formula includes, by weight percentage:
[0056] 10-15% kaolin, 18-25% potassium feldspar, 5-10% frit, 10-13% barium carbonate, 18-30% calcite, 4-8% zinc oxide, 18-25% quartz; wherein the sum of the weight percentages of the various components is 100%.
[0057] The second raw material formula, measured by weight percentage, includes:
[0058] Potash feldspar 45-55%, frit 6-10%, barium carbonate 10-18%, calcite 20-25%, zinc oxide 3-6%, quartz 12-18%; wherein the sum of the weight percentages of the various components is 100%.
[0059] Specifically, the raw material formula of the embodiment of the present application includes two types to adapt to different kiln temperatures during secondary calcination. In the sintered material prepared by the first raw material formula, there will be two types of crystals synthesized by the solid phase reaction method. One is to generate a large number of barium crystalline crystals, which serve as the main crystal phase in the microcrystalline ceramic glaze. The presence of a large amount of crystals in the glaze can make the glaze matte; the other is to generate zinc orthoclase and wollastonite. When finely ground corundum (α-Al2O3) is introduced into the formula, a solid phase reaction occurs with it to generate microcrystals such as barium crystalline and calcium feldspar, making the glaze matte. The phase analysis results are shown in Table 3. The diffraction pattern of the sintered material prepared by the first raw material formula is shown in Table 3. Figure 2 shown.
[0060] Table 3 Phase analysis test results
[0061]
[0062] The raw material formula of the embodiment of the present application is simple and easy to master. In this formula system, the sintering material accounts for 85±5wt%, and the kaolin is 8-12wt%. When fired in a common ceramic tile kiln, the glaze has a gloss of 20±10 degrees, a smooth and delicate glaze surface, and a surface roughness of less than 1.0 micron.
[0063] On this basis, if the glaze is too glossy, a small amount of ultrafine corundum, ultrafine alumina powder, calcined kaolin, etc. can be added to reduce the gloss. The order of the intensity of reducing the gloss of these three raw materials is: ultrafine corundum ≈ ultrafine alumina powder ﹥ ﹥ calcined kaolin. The amount of each raw material added can be fine-tuned according to the specific situation.
[0064] On this basis, if the glaze gloss is too low, a small amount of potassium feldspar, sodium feldspar, wollastonite, calcined talc, etc. can be added to improve the gloss. The order of the strength of these four raw materials in improving gloss is: wollastonite > sodium feldspar > potassium feldspar > calcined talc. The amount of each raw material added can be fine-tuned according to the specific situation. The trace addition of the above two types of raw materials will not make a significant difference to the surface roughness of the glaze.
[0065] In this embodiment, the first raw material formula specifically includes, by weight percentage, kaolin 14%, potassium feldspar 24%, frit 6%, barium carbonate 12%, calcite 20%, zinc oxide 5%, and quartz 19%. The second raw material formula specifically includes, by weight percentage, potassium feldspar 45%, frit 6%, barium carbonate 11%, calcite 21%, zinc oxide 5%, and quartz 12%.
[0066] The embodiment of the present application makes the glaze formula of microcrystalline ceramic glaze ceramic tiles with a gloss of less than 20 degrees very simple, with low surface roughness, no defects such as pinhole bubbles, wide adaptability to kiln firing temperature, and low requirements for glaze layer thickness. It is of great significance to improve the quality and stabilize the quality of this type of ceramic tile products.
[0067] In one embodiment of the present application, the chemical components of the frit include, by weight percentage:
[0068] Loss on ignition 0.3-1.2%, SiO2 50-60%, Al2O3 8-12%, Fe2O3 0.1-0.5%, TiO20.08-0.2%, CaO 16-20%, MgO 5-8%, K2O 3.5-5%, Na2O 2-3%, ZnO 0.3-0.6%, B2O3 0.1-0.3%, BaO0.6-1.5%; wherein the sum of the weight percentages of each component is 100%.
[0069] Specifically, the chemical composition analysis of the frit is: loss on ignition 1.02%, SiO2 52.76%, Al2O3 11.93%, Fe2O3 0.11%, TiO2 0.2%, CaO 18.46%, MgO 6.82%, K2O 4.19%, Na2O 2.05%, ZnO 0.6%, B2O3 0.18%, and BaO 1.31%.
[0070] In an embodiment of the present application, the step S100 specifically includes: after mixing the ingredients according to a predetermined raw material formula, adding sodium carboxymethyl cellulose, sodium tripolyphosphate and water for wet ball milling, grinding to a fineness of 0.1 to 0.3% with a 325-mesh sieve residue, and obtaining a glaze powder after spray drying; or, after mixing the ingredients according to a predetermined raw material formula, conveying them to a Raymond mill for fine grinding to a fineness of 0.1 to 0.3% with a 325-mesh sieve residue, to obtain a glaze powder.
[0071] Specifically, the embodiments of the present application give priority to dry ball milling, and wet ball milling is the second choice. In wet ball milling, 0.1%-0.3% sodium carboxymethyl cellulose (CMC), 0.3%-0.6% sodium tripolyphosphate, and 40%-46% water are added, and the mixture is ground to a fineness of 0.1-0.3% on a 325-mesh sieve, and spray-dried to obtain a glaze powder to be fired. Wet ball milling is beneficial to improving the convenience and efficiency of iron removal in the glaze slurry during processing. In dry ball milling, no additives are added, and the mixture is transported to a Raymond mill for fine grinding to a fineness of 0.1-0.3% on a 325-mesh sieve, and then fired. The energy consumption cost of dry ball milling is relatively low.
[0072] like Figure 1 As shown, the preparation method of the secondary sintered microcrystalline ceramic glaze also includes:
[0073] Step S200: calcining the glaze powder material to obtain a sintered material.
[0074] Specifically, the embodiment of the present application is a loose sintering of bulk materials. The strength of the particles after sintering is not high and it is very easy to grind finely, so there is no need for crushing and coarse grinding.
[0075] In the embodiment of the present application, the step S200 specifically includes: calcining the glaze powder material at a temperature of 1000-1150° C. to obtain a sintered material.
[0076] Specifically, the finely ground glaze powder is calcined at a temperature of 1000-1150°C and kept warm for 1 hour at high temperature. The sintering degree of the sintering material has a great influence on its use in the glaze. If the sintering degree of the sintering material is high, the initial melting point of the sintering material is low, and the microcrystalline ceramic glaze is prone to premature pore closure at high temperature, resulting in defects such as pinholes and prickly heat on the glaze surface. If the sintering degree of the sintering material is low, the carbonate cannot fully react with silicon, aluminum, etc., and calcium, barium and other ions are dissolved in water, resulting in a strong thixotropy of the glaze slurry and a large flow rate, which does not meet the requirements of the glazing process. Therefore, the embodiment of the present application also controls the sintering degree of the sintering material.
[0077] To measure the degree of sintering, the material to be fired can be adjusted to a moisture content of 6-8%, pressed into a cake at a pressure of 35MPa, fired at the same time as the material to be fired, and calcined at 1000-1150℃ for use. The water absorption rate of the cake out of the kiln is between 20% and 25%, which can largely ensure the high initial melting point of the material, and ensure that it will not cause the glaze slurry to have a strong thixotropic flow rate when added to the glaze, and is easy to use for glazing.
[0078] In the microcrystalline ceramic glaze of the embodiments of the present application, the carbonates are fully reacted after calcination at 1000-1150°C, the silicon and aluminum content in the sintered material is not very high, the microcrystalline ceramic glaze has a high initial melting point during the firing process and a low high-temperature viscosity, so the use of the sintered material in the glaze will not cause the glaze surface to close prematurely, and the gas in the body can be discharged smoothly; since the silicon and aluminum content in the formula is not high, the glaze has a low viscosity at high temperature and can easily fill the exhaust holes, thereby eliminating glaze defects such as pinholes and prickly heat.
[0079] like Figure 1 As shown, the preparation method of the secondary sintered microcrystalline ceramic glaze also includes:
[0080] Step S300, mixing ingredients according to a predetermined microcrystalline ceramic glaze formula and grinding them into glaze slurry, wherein the microcrystalline ceramic glaze formula includes the sintering material.
[0081] Specifically, the microcrystalline ceramic glaze firing process includes: batching → wet ball milling → testing fineness and flow rate → adjusting flow rate → discharging slurry → conveying to the glaze line for glazing → firing → obtaining microcrystalline ceramic glaze ceramic tile products. The fineness of the glaze slurry is 0.2-0.4% of the 325 mesh sieve residue, and the slurry flow rate is about 35 seconds.
[0082] In an embodiment of the present application, the formula of the microcrystalline ceramic glaze includes, by weight percentage: 8-12% kaolin, 60-90% sintering material, 0-5% ultrafine corundum powder, 0-5% ultrafine alumina powder, 0-8% calcined kaolin, 0-30% potassium feldspar, 0-20% sodium feldspar, 0-5% wollastonite, 0-8% burned talc, 0-10% dolomite, 0-12% calcite, 0-8% barium carbonate, 0-5% strontium carbonate, and 0-8% zinc oxide; wherein the sum of the weight percentages of each component is 100%.
[0083] Specifically, the above sintered materials are mixed with kaolin, calcined kaolin, potassium feldspar, sodium feldspar, corundum (or alumina), wollastonite, burned talc, etc. according to a formula and finely ground into glaze slurry, which is glazed on inkjet-printed ceramic tile blanks and fired at 1150-1230°C to obtain microcrystalline ceramic glazed tiles.
[0084] like Figure 1 As shown, the preparation method of the secondary sintered microcrystalline ceramic glaze also includes:
[0085] Step S400: applying the glaze slurry to the brick and then performing secondary calcination to obtain a microcrystalline ceramic glaze.
[0086] Specifically, the microcrystalline ceramic glaze in the embodiment of the present application is a microcrystalline ceramic glaze covering the surface of the brick, with the glaze gloss adjustable between 5 and 20 degrees and the glaze surface roughness below 1.0 micron, and the main crystal phase of the microcrystals is barium cryolite.
[0087] In the embodiment of the present application, the step S400 specifically includes: after applying the glaze slurry to the brick, performing secondary calcination at a temperature of 1140-1230° C. to obtain a microcrystalline ceramic glaze.
[0088] Specifically, the glaze slurry bell jar is poured onto the brick blank, and then put into the kiln for firing along with the brick blank. After being fired at 1140-1230° C., a smooth and low-gloss microcrystalline ceramic glaze is formed.
[0089] In a specific embodiment of the present application, step S400 specifically includes: if the glaze slurry is prepared from a sintered material prepared from a first raw material formula, then after the glaze slurry is applied to the brick blank, a secondary calcination is carried out under a temperature condition of 1190℃-1230℃ to obtain a microcrystalline ceramic glaze; if the glaze slurry is prepared from a sintered material prepared from a second raw material formula, then after the glaze slurry is applied to the brick blank, a secondary calcination is carried out under a temperature condition of 1140℃-1170℃ to obtain a microcrystalline ceramic glaze.
[0090] Specifically, the first raw material formula and the second raw material formula are used for different kiln temperatures. The first raw material formula is used when the kiln temperature is high, and the applicable range is 1190℃-1230℃. The second raw material formula is used when the kiln temperature is low, and the applicable range is 1140℃-1170℃. The two can also be mixed.
[0091] The microcrystalline ceramic glaze prepared in the embodiment of the present application has a wide firing range and wider adaptability. The microcrystals in the microcrystalline ceramic glaze are formed during the first sintering, and will not be completely melted during the second sintering (the crystals in the glaze, unless they reach their melting temperature or are melted into glass by the low-temperature glass phase, still exist in the form of crystals). Therefore, there are a large number of tiny crystals in the glaze, making the glaze matte. During the second sintering process of the microcrystalline ceramic glaze, from the thermal analysis diagram of the glaze, there is no obvious endothermic peak, only an exothermic peak. It does not need to go through the process of first melting and then crystallization. Therefore, it is minimally affected by the kiln temperature, has a wide firing range, and is conducive to the stability of production.
[0092] The microcrystalline ceramic glaze of the embodiment of the present application has a wide firing range, which is mainly reflected in two aspects.
[0093] First, it can adapt to a wider range of kiln firing temperatures.
[0094] Table 4 Firing effect of the first raw material formula in different kilns
[0095]
[0096] The microcrystalline ceramic glaze of the embodiment of the present application is fired in kilns with a kiln temperature difference of 30°C, and the glaze surface is equally fine and smooth, and the maximum difference in glossiness is only 2 degrees, and the surface roughness is less than 1.0 micron. In the experiment of microcrystalline ceramic glaze, the color of the glaze printed by inkjet printing is good, and the transparency is excellent, which improves the production stability.
[0097] Second, it can adapt to different glaze layer thicknesses.
[0098] As is known to all, the effect of crystallized glaze is greatly affected by the thickness of the glaze layer. However, the thickness of the glaze layer of the microcrystalline ceramic glaze of the present invention has little effect on the crystallization effect and thus little effect on the glaze gloss, as shown in the following table.
[0099] Table 5 Glaze effect of different thickness of scraping the first raw material formula and firing on J1 line
[0100]
[0101] Table 6 Glaze effect of different thickness of scraping the first raw material formula on the Q6 line
[0102]
[0103] Table 7 Glaze effect of different thickness of scraping the first raw material formula on the Q5 line
[0104]
[0105] The embodiments of the present application achieve the following effects:
[0106] First, the microcrystalline ceramic glaze prepared in the embodiment of the present application has a glaze gloss as low as below 10 degrees, a surface roughness as low as 0.6 microns, and a glaze surface free of pinholes and prickly heat. The glaze effect is less affected by the kiln temperature and the thickness of the glaze layer, and the glaze formula has good adaptability and a wide firing range.
[0107] Second, the microcrystalline ceramic glaze prepared in the embodiment of the present application has a simple formula structure and wide adaptability, and is very easy for technicians to master and use.
[0108] Third, the sintering material of the embodiment of the present application has a low sintering temperature, which saves energy for the society; the structure is loose after sintering, which saves processing costs.
[0109] Fourthly, the embodiment of the present application replaces the high-temperature molten material (microcrystalline frit) with the low-temperature sintering material, thereby realizing the substitutability of the glaze preparation.
[0110] A second aspect of the present application provides a microcrystalline ceramic glaze, which is prepared based on the preparation method of the microcrystalline ceramic glaze by secondary sintering as described above.
[0111] A third aspect of the present application provides a microcrystalline ceramic glazed tile, wherein the microcrystalline ceramic glaze as described above is applied on the microcrystalline ceramic glaze tile.
[0112] The present invention provides a microcrystalline ceramic glaze with secondary sintering and a preparation method thereof, and a microcrystalline ceramic glaze brick, the method comprising: mixing ingredients according to a predetermined raw material formula and then ball milling to obtain a glaze powder; calcining the glaze powder to obtain a sintering material; mixing ingredients according to a predetermined microcrystalline ceramic glaze formula and grinding into a glaze slurry, wherein the microcrystalline ceramic glaze formula includes the sintering material; applying the glaze slurry to a brick blank and then calcining it for a secondary time to obtain a microcrystalline ceramic glaze. The microcrystals in the microcrystalline ceramic glaze prepared by the present invention are formed during the first sintering, and will not be completely melted during the secondary sintering, and do not need to go through a process of first melting and then crystallization, so they are minimally affected by the kiln temperature, have a wide firing range, and are conducive to the stability of production.
[0113] It should be understood that the application of the present invention is not limited to the above examples. For ordinary technicians in this field, improvements or changes can be made based on the above description. All these improvements and changes should fall within the scope of protection of the claims attached to the present invention.
Claims
1. A method for preparing a twice-sintered microcrystalline ceramic glaze, characterized in that: The method comprises: After mixing the raw materials according to the predetermined formula, ball milling is performed to obtain glaze powder; calcining the glaze powder material to obtain a sintered material; Mixing ingredients according to a predetermined microcrystalline ceramic glaze formula and grinding them into glaze slurry, wherein the microcrystalline ceramic glaze formula includes the sintering material; The glaze slurry is applied to the brick and then secondary calcined to obtain a microcrystalline ceramic glaze.
2. The method for preparing the secondary sintered microcrystalline ceramic glaze according to claim 1, characterized in that: The raw material formula includes a first raw material formula and a second raw material formula, wherein the first raw material formula includes, by weight percentage: Kaolin 10-15%, potassium feldspar 18-25%, frit 5-10%, barium carbonate 10-13%, calcite 18-30%, zinc oxide 4-8%, quartz 18-25%; The second raw material formula, calculated by weight percentage, includes: Potassium feldspar 45-55%, frit 6-10%, barium carbonate 10-18%, calcite 20-25%, zinc oxide 3-6%, quartz 12-18%.
3. The method for preparing the secondary sintered microcrystalline ceramic glaze according to claim 2, characterized in that: The chemical components of the frit include, by weight percentage: Loss on ignition 0.3-1.2%, SiO2 50-60%, Al2O3 8-12%, Fe2O3 0.1-0.5%, TiO20.08-0.2%, CaO 16-20%, MgO 5-8%, K2O 3.5-5%, Na2O 2-3%, ZnO 0.3-0.6%, B2O3 0.1-0.3%, BaO0.6-1.5%.
4. The method for preparing the secondary sintered microcrystalline ceramic glaze according to claim 1, characterized in that: The process of preparing the raw materials according to a predetermined raw material formula and then ball milling the raw materials to obtain a glaze powder material comprises: After mixing the ingredients according to the predetermined raw material formula, sodium carboxymethyl cellulose, sodium tripolyphosphate and water are added for wet ball milling to a fineness of 0.1-0.3% of the residue on a 325-mesh sieve, and then spray-dried to obtain a glaze powder; Alternatively, the raw materials are mixed according to a predetermined formula and then conveyed to a Raymond mill for fine grinding to a fineness of 0.1-0.3% of the residue on a 325-mesh sieve to obtain a glaze powder.
5. The method for preparing the twice-sintered microcrystalline ceramic glaze according to claim 1, characterized in that: The glaze powder is calcined to obtain a sintered material, comprising: The glaze powder material is calcined at a temperature of 1000-1150° C. to obtain a sintered material.
6. The method for preparing the twice-sintered microcrystalline ceramic glaze according to claim 1, characterized in that: The microcrystalline ceramic glaze formula comprises, by weight percentage: 8-12% kaolin, 60-90% sintering material, 0-5% ultrafine corundum powder, 0-5% ultrafine alumina powder, 0-8% calcined kaolin, 0-30% potassium feldspar, 0-20% sodium feldspar, 0-5% wollastonite, 0-8% burned talc, 0-10% dolomite, 0-12% calcite, 0-8% barium carbonate, 0-5% strontium carbonate, and 0-8% zinc oxide.
7. The method for preparing the twice-sintered microcrystalline ceramic glaze according to claim 1, characterized in that: The glaze slurry is applied to the brick and then secondary calcined to obtain a microcrystalline ceramic glaze, comprising: After the glaze slurry is applied to the brick, secondary calcination is performed at a temperature of 1140-1230° C. to obtain a microcrystalline ceramic glaze.
8. The method for preparing the twice-sintered microcrystalline ceramic glaze according to claim 2, characterized in that: The glaze slurry is applied to the brick and then secondary calcined to obtain a microcrystalline ceramic glaze, comprising: If the glaze slurry is prepared from the sintered material prepared from the first raw material formula, the glaze slurry is applied to the brick blank and then secondary calcined at a temperature of 1190° C. to 1230° C. to obtain a microcrystalline ceramic glaze; If the glaze slurry is prepared from a sintered material prepared from the second raw material formula, the glaze slurry is applied to the brick and then secondary calcined at a temperature of 1140° C. to 1170° C. to obtain a microcrystalline ceramic glaze.
9. A microcrystalline ceramic glaze, characterized in that: The microcrystalline ceramic glaze is prepared based on the preparation method of the secondary sintered microcrystalline ceramic glaze as described in any one of claims 1 to 8.
10. A microcrystalline ceramic glazed tile, characterized in that: The microcrystalline ceramic glaze tile is applied with the microcrystalline ceramic glaze as claimed in claim 9.
Citation Information
Patent Citations
Glaze slip for sanitary ceramics and preparation method for glaze slip
CN102584341A
Ceramic glaze and preparation method thereof
CN107417117A
A method for preparing ceramic crystalline glaze using steel slag
CN114933413A
Cited By
Quick firing glaze powder as well as preparation method and application thereof
CN119822641A