Production process of silver mirror

By simplifying the silver mirror production process, using steps such as chemical copper plating, silver plating, and annealing, a silver film with high reflectivity and low dispersion is formed, and a protective film is formed on the surface of the silver layer. This solves the problem of poor corrosion resistance of silver mirrors in existing technologies and achieves high reflectivity, low dispersion, and environmentally friendly production.

CN118878221AInactive Publication Date: 2024-11-01杭州港盛卫浴有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410901159.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-05
Publication Date
2024-11-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing silver mirror manufacturing processes are complex and produce silver mirrors with poor corrosion resistance, which affects their service life.

Method used

The process involves steps such as chemical copper plating, silver plating, annealing, curing, mirror coating with back paint, and edge grinding. This includes selecting appropriate copper plating agents and electroplating silver parameters to form a silver film with high reflectivity and low dispersion. A complex protective film is then formed on the surface of the silver layer, and environmentally friendly electrostatic spraying UV paint is used.

Benefits of technology

The resulting silver mirrors have a reflectivity of over 99%, a low dispersion coefficient, strong corrosion resistance, extended service life, and an environmentally friendly production process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118878221A_ABST
    Figure CN118878221A_ABST
Patent Text Reader

Abstract

According to the technical scheme, the production technology is characterized by comprising the following steps that S1, raw materials are prepared, specifically, the prepared raw materials comprise pure silver and glass, the pure silver is made into a silver plate through the casting technology and other technologies, and the glass is made into a lens through the cleaning, cutting and edge grinding technologies; s2, chemical copper plating: carrying out chemical copper plating treatment on the surface of the lens; s3, silver plating: forming a layer of silver film on the surface of the lens; s4, annealing: putting the silver-plated lens into a high-temperature furnace for annealing treatment to eliminate stress on the surface of the lens; s5, curing: cleaning the silver plating layer, passivating the silver plating layer and immersing the silver plating layer into an organic film; s6, coating back paint on the mirror surface: spraying the back paint on the back surface of the lens; s7, mirror surface edge grinding is conducted, specifically, the annealed lens is subjected to edge grinding treatment, so that the edge of the lens is flat and smooth; and S8, mirror surface cleaning and inspection: cleaning and inspecting the edged lens to ensure that the surface of the lens is clean and flawless and meets the quality standard.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of glass mirror processing, and more specifically, to a production process of a silver mirror. Background Art

[0002] A mirror is a glass or metal product made of glass, silver, etc. with regular reflective properties and a polished surface and coated with a metal reflective film. It has the advantages of high reflectivity, low dispersion, and corrosion resistance. Mirrors are divided into plane mirrors and curved mirrors, among which curved mirrors are divided into concave mirrors and convex mirrors. The mirrors commonly used in our lives are dressing mirrors, which are made of silver mirrors, which can also be called silver-coated glass mirrors.

[0003] The existing Chinese patent with publication number CN113955949A discloses a production process of a silver mirror, which relates to the field of mirror production and manufacturing, and aims to solve the problems of short service life and low reflectivity of silver mirrors. The key points of its technical solution are: a production process of a silver mirror, including: glass cleaning and polishing; sensitization; supersensitization; silver plating; passivation; preheating; primer pouring; primer baking; epoxy resin coating liquid spraying; topcoat pouring; air cooling; pickling surface; surface cleaning; drying. The production process of a silver mirror of the present invention can ensure that the silver layer has a long durability, high reflectivity, and a long service life.

[0004] Another example is the Chinese patent with the existing publication number CN101549960B, which discloses a silver mirror production process and equipment for non-planar glass: partially protect the non-processed surface of the non-planar glass to be processed; clean; sensitize; silver-plated: after positioning the non-planar glass to be processed, press down the frame, enclose the non-planar glass to be processed in the frame, and spray the silver nitrate mixed liquid into the frame, so that the liquid completely submerges the highest point of the non-planar glass to be processed, so as to promote a full chemical reaction between the liquid and the glass surface; after a period of reaction, lift the frame and discharge the reacted liquid; rinse the liquid, blow air to remove water, and dry with hot air; spray protective paint and dry; cool the mirror surface and cut the material. This production process is applied to the production of the reflective layer of the non-planar shuttle mirror. Since the frame is used in the production equipment, the production cost is greatly saved, the production efficiency is improved, and large-scale production line production can be realized.

[0005] The above-mentioned patent and the current technology have some advantages, but also some disadvantages, such as: the above-mentioned process is relatively complicated, and the corrosion resistance of the generated silver mirror is poor, which affects the service life. Summary of the invention

[0006] In view of the shortcomings of the prior art, the object of the present invention is to provide a production process for a silver mirror to solve the problems raised by the background technology.

[0007] The above technical objectives of the present invention are achieved through the following technical solutions: A production process of a silver mirror comprises the following steps:

[0008] S1. Raw material preparation: The raw materials prepared include pure silver and glass. Pure silver is made into silver plates through casting and other processes, and glass is made into lenses through cleaning, cutting and edge grinding processes;

[0009] S2, chemical copper plating: chemical copper plating is performed on the surface of the lens;

[0010] S3, Silver plating: Form a layer of silver film on the surface of the lens;

[0011] S4, annealing: putting the silver-plated lens into a high-temperature furnace for annealing to eliminate the stress on the lens surface;

[0012] S5, curing: including cleaning the silver-plated layer, passivating the silver-plated layer and dipping the organic film;

[0013] S6, mirror coating back paint: spray back paint on the back of the lens;

[0014] S7, mirror edge grinding: the annealed lens is edged to make the edge of the lens flat and smooth;

[0015] S8. Mirror cleaning and inspection: Clean and inspect the edged lenses to ensure that the lens surface is clean, free of defects and meets quality standards.

[0016] Preferably, in S2, a first copper precipitate and a second copper precipitate are selected for standby use, and the first copper precipitate, the second copper precipitate and deionized water are mixed in a mass ratio of 1:1:2, and then the lens is degreased and activated by pickling for 3 minutes. During the copper plating process, a first copper precipitate and sodium hydroxide are added, and the pH value is tested and adjusted to 12-13. According to the copper plating loading ratio of 2-4 square decimeters / liter, the copper plating temperature is 30-45°C, and continuous stirring and circulating filtration are carried out during the copper plating process to keep the plating solution transparent and free of impurities. After the copper plating is completed, the lens is cleaned with ultrasound.

[0017] Preferably, the first copper plating agent is copper plating solution HSECu-801, and the second copper plating agent is Cu800 copper plating supplement.

[0018] Preferably, when S3 is silver-plated, an electroplating silver process is adopted, and the parameters of the electroplating silver are: the electroplating silver water is: main salt silver nitrate 5-30g / L, potassium silver cyanide 80-130g / L, complexing agent ammonium acetate 80-130g / L, potassium hydroxide 40-90mL / L, brightener 5-20mL / L, electroplating parameters are pH 9-10, temperature 30-40°C, current 20-40A, specific gravity 20-25, time 40-60min, and ES-02A brightener is added during silver plating.

[0019] Preferably, the S3 is subjected to a galvanizing operation before silver plating, and the process parameters of the galvanizing operation are: using EN-AL-216 zinc immersion solution, the concentration is 200-300ml / L, the temperature is 20-40°C, the time is 10-20S, and the Bemei degree is 14-16Be.

[0020] Preferably, when the S5 is solidified, the silver-plated layer is cleaned by deionization and dried at 50-60°C; when the silver-plated layer is passivated, it is treated with a dichromate solution to form a silver oxide and silver chromate film on the surface; when the organic film is immersed, one of TX, TF, SN, and LP-98S organic substances is coated on the surface of the silver layer to produce a complex protective film on the surface of the silver layer.

[0021] Preferably, when the S6 is mirror-coated with back paint, electrostatic spraying of UV paint is adopted, the electrostatic pressure is controlled at 60-90KV, the flow rate pressure is set at 0.3-0.5MPa, the atomization pressure is set at 0.05-0.15MPa, the nozzle is 200-300mm away from the workpiece, the nozzle diameter is 14-18mm, and UV curing operation is performed after electrostatic spraying.

[0022] Preferably, the S8 adopts a sampling inspection method during the mirror inspection, and the inspection parameters include: moisture and heat resistance, neutral salt spray resistance, optical properties, thickness, dimensional tolerance, diagonal difference and appearance quality.

[0023] Preferably, after the S8 detects that the coating is unqualified, it uses 50% by volume or more nitric acid to soak until the coating is completely removed, and then re-performs the coating operation.

[0024] In summary, the present invention has the following beneficial effects: the production process of the present invention is simple, the process is short, and the production cost is low; the silver mirror produced by the present invention has a high reflectivity, and the reflectivity of the silver mirror is as high as more than 99%; the present invention also has a low dispersion characteristic, and the dispersion coefficient of the silver mirror is very low, which is only about one tenth of that of an ordinary glass lens, and can effectively avoid the chromatic aberration caused by the different refractive indices of light of different wavelengths, and provide a more realistic visual effect; in addition, the surface of the silver mirror of the present invention has strong corrosion resistance, and the silver film and back paint on the surface of the silver mirror have good corrosion resistance, which can maintain the reflectivity and clarity of the lens for a long time and extend the service life of the lens; in addition, the production process of the present invention is more environmentally friendly, and no harmful substances are used in the production process of the silver mirror, which meets environmental protection requirements. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is a flow chart of the present invention. DETAILED DESCRIPTION

[0026] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] Example 1

[0028] refer to Figure 1 , a production process of a silver mirror, comprising the following steps:

[0029] S1. Raw material preparation: The raw materials prepared include pure silver and glass. Pure silver is made into silver plates through casting and other processes, and glass is made into lenses through cleaning, cutting and edge grinding processes;

[0030] S2, chemical copper plating: chemical copper plating is performed on the surface of the lens;

[0031] S3, Silver plating: Form a layer of silver film on the surface of the lens;

[0032] S4, annealing: putting the silver-plated lens into a high-temperature furnace for annealing to eliminate the stress on the lens surface;

[0033] S5, curing: including cleaning the silver-plated layer, passivating the silver-plated layer and dipping the organic film;

[0034] S6, mirror coating back paint: spray back paint on the back of the lens;

[0035] S7, mirror edge grinding: the annealed lens is edged to make the edge of the lens flat and smooth;

[0036] S8. Mirror cleaning and inspection: Clean and inspect the edged lenses to ensure that the lens surface is clean, free of defects and meets quality standards.

[0037] Among them, in S2, a copper precipitate of one and a copper precipitate of two are selected for standby use, and the copper precipitate of one, the copper precipitate of two and deionized water are mixed in a mass ratio of 1:1:2, and then the lens is degreased and activated by pickling for 3 minutes. During the copper plating process, a copper precipitate of one and sodium hydroxide are added, and the pH value is tested and adjusted to 12. According to the copper plating loading ratio of 2 square decimeters / liter, the copper plating temperature is 30°C, and continuous stirring and circulating filtration are carried out during the copper plating process to keep the plating solution transparent and free of impurities. After the copper plating is completed, the lens is cleaned with ultrasound.

[0038] The first copper plating agent is HSECu-801 copper plating solution, and the second copper plating agent is Cu800 copper plating supplement.

[0039] Among them, the S3 adopts the electroplating silver process when silver plating, and the parameters of the electroplating silver are: the electroplating silver water is: main salt silver nitrate 5g / L, potassium silver cyanide 130g / L, complexing agent ammonium acetate 80g / L, potassium hydroxide 40mL / L, brightener 5mL / L, electroplating parameters are pH10, temperature 30°C, current 20A, specific gravity 20, time 40min, and ES-02A brightener is added during silver plating.

[0040] Wherein, the S3 is subjected to a galvanizing operation before silver plating, and the process parameters of the galvanizing operation are: using EN-AL-216 zinc immersion solution, the concentration is 200ml / L, the temperature is 20°C, the time is 10S, and the degree of beauty is 16Be.

[0041] Among them, when the S5 is solidified, deionization is used for cleaning when cleaning the silver-plated layer, and it is dried at 50-60°C; when passivating the silver-plated layer, it is treated with a dichromate solution to form a silver oxide and silver chromate film on the surface; when dipping the organic film, LP-98S organic matter is coated on the surface of the silver layer to produce a complex protective film on the surface of the silver layer.

[0042] Among them, when the S6 is mirror-coated with back paint, electrostatic spraying of UV paint is adopted, the electrostatic pressure is controlled at 60KV, the flow rate pressure is set at 0.3MPa, the atomization pressure is set at 0.05MPa, the nozzle is 200mm away from the workpiece, the nozzle diameter is 18mm, and UV curing operation is performed after electrostatic spraying.

[0043] Among them, the S8 adopts a sampling inspection method during the mirror inspection, and the inspection parameters include: moisture and heat resistance, neutral salt spray resistance, optical properties, thickness, dimensional tolerance, diagonal difference and appearance quality.

[0044] Wherein, after the coating is found unqualified in the inspection, S8 uses nitric acid with a volume ratio of more than 50% to soak until the coating is completely removed, and then the coating operation is repeated.

[0045] Among them, the present invention has the following beneficial effects: the production process of the present invention is simple, the process is short, and the production cost is low; the silver mirror produced by the present invention has high reflectivity, and the reflectivity of the silver mirror is as high as more than 99%; the present invention also has low dispersion characteristics, and the dispersion coefficient of the silver mirror is very low, which is only about one tenth of that of ordinary glass lenses, and can effectively avoid chromatic aberration caused by different refractive indices of light of different wavelengths, and provide a more realistic visual effect; in addition, the surface of the silver mirror of the present invention has strong corrosion resistance, and the silver film and back paint on the surface of the silver mirror have good corrosion resistance, which can maintain the reflectivity and clarity of the lens for a long time and extend the service life of the lens; in addition, the production process of the present invention is more environmentally friendly, and no harmful substances are used in the production process of the silver mirror, which meets environmental protection requirements.

[0046] Example 2

[0047] refer to Figure 1 , a production process of a silver mirror, comprising the following steps:

[0048] S1. Raw material preparation: The raw materials prepared include pure silver and glass. Pure silver is made into silver plates through casting and other processes, and glass is made into lenses through cleaning, cutting and edge grinding processes;

[0049] S2, chemical copper plating: chemical copper plating is performed on the surface of the lens;

[0050] S3, Silver plating: Form a layer of silver film on the surface of the lens;

[0051] S4, annealing: putting the silver-plated lens into a high-temperature furnace for annealing to eliminate the stress on the lens surface;

[0052] S5, curing: including cleaning the silver-plated layer, passivating the silver-plated layer and dipping the organic film;

[0053] S6, mirror coating back paint: spray back paint on the back of the lens;

[0054] S7, mirror edge grinding: the annealed lens is edged to make the edge of the lens flat and smooth;

[0055] S8. Mirror cleaning and inspection: Clean and inspect the edged lenses to ensure that the lens surface is clean, free of defects and meets quality standards.

[0056] Among them, in S2, a copper precipitate of one and a copper precipitate of two are selected for standby use, and the copper precipitate of one, the copper precipitate of two and deionized water are mixed in a mass ratio of 1:1:2, and then the lens is degreased and activated by pickling for 3 minutes. During the copper plating process, a copper precipitate of one and sodium hydroxide are added, and the pH value is tested and adjusted to 13. According to the copper plating loading ratio of 4 square decimeters per liter, the copper plating temperature is 30°C, and continuous stirring and circulating filtration are carried out during the copper plating process to keep the plating solution transparent and free of impurities. After the copper plating is completed, the lens is cleaned with ultrasound.

[0057] The first copper plating agent is HSECu-801 copper plating solution, and the second copper plating agent is Cu800 copper plating supplement.

[0058] Among them, the S3 adopts the electroplating silver process when silver plating, and the parameters of the electroplating silver are: the electroplating silver water is: main salt silver nitrate 20g / L, potassium silver cyanide 100g / L, complexing agent ammonium acetate 110g / L, potassium hydroxide 70mL / L, brightener 15mL / L, electroplating parameters are pH10, temperature 33°C, current 28A, specific gravity 22, time 46min, and ES-02A brightener is added during silver plating.

[0059] Wherein, the S3 is subjected to a galvanizing operation before silver plating, and the process parameters of the galvanizing operation are: using EN-AL-216 zinc immersion solution, the concentration is 240ml / L, the temperature is 30°C, the time is 14S, and the Bemei degree is 14-16Be.

[0060] Among them, when the S5 is solidified, deionization is used for cleaning the silver-plated layer and it is dried at 50-60°C; when the silver-plated layer is passivated, it is treated with a dichromate solution to form a silver oxide and silver chromate film on the surface; when the organic film is immersed, TF is coated on the surface of the silver layer to produce a complex protective film on the surface of the silver layer.

[0061] Among them, when the S6 is mirror-coated with back paint, electrostatic spraying of UV paint is adopted, the electrostatic pressure is controlled at 70KV, the flow rate pressure is set at 0.4MPa, the atomization pressure is set at 0.15MPa, the nozzle is 300mm away from the workpiece, the nozzle diameter is 18mm, and UV curing operation is performed after electrostatic spraying.

[0062] Among them, the S8 adopts a sampling inspection method during the mirror inspection, and the inspection parameters include: moisture and heat resistance, neutral salt spray resistance, optical properties, thickness, dimensional tolerance, diagonal difference and appearance quality.

[0063] Wherein, after the coating is found unqualified in the inspection, S8 uses nitric acid with a volume ratio of more than 50% to soak until the coating is completely removed, and then the coating operation is repeated.

[0064] Among them, the present invention has the following beneficial effects: the production process of the present invention is simple, the process is short, and the production cost is low; the silver mirror produced by the present invention has high reflectivity, and the reflectivity of the silver mirror is as high as more than 99%; the present invention also has low dispersion characteristics, and the dispersion coefficient of the silver mirror is very low, which is only about one tenth of that of ordinary glass lenses, and can effectively avoid chromatic aberration caused by different refractive indices of light of different wavelengths, and provide a more realistic visual effect; in addition, the surface of the silver mirror of the present invention has strong corrosion resistance, and the silver film and back paint on the surface of the silver mirror have good corrosion resistance, which can maintain the reflectivity and clarity of the lens for a long time and extend the service life of the lens; in addition, the production process of the present invention is more environmentally friendly, and no harmful substances are used in the production process of the silver mirror, which meets environmental protection requirements.

[0065] Example 3

[0066] refer to Figure 1 , a production process of a silver mirror, comprising the following steps:

[0067] S1. Raw material preparation: The raw materials prepared include pure silver and glass. Pure silver is made into silver plates through casting and other processes, and glass is made into lenses through cleaning, cutting and edge grinding processes;

[0068] S2, chemical copper plating: chemical copper plating is performed on the surface of the lens;

[0069] S3, Silver plating: Form a layer of silver film on the surface of the lens;

[0070] S4, annealing: putting the silver-plated lens into a high-temperature furnace for annealing to eliminate the stress on the lens surface;

[0071] S5, curing: including cleaning the silver-plated layer, passivating the silver-plated layer and dipping the organic film;

[0072] S6, mirror coating back paint: spray back paint on the back of the lens;

[0073] S7, mirror edge grinding: the annealed lens is edged to make the edge of the lens flat and smooth;

[0074] S8. Mirror cleaning and inspection: Clean and inspect the edged lenses to ensure that the lens surface is clean, free of defects and meets quality standards.

[0075] Among them, in S2, a copper precipitate of one and a copper precipitate of two are selected for standby use, and the copper precipitate of one, the copper precipitate of two and deionized water are mixed in a mass ratio of 1:1:2, and then the lens is degreased and activated by pickling for 3 minutes. During the copper plating process, a copper precipitate of one and sodium hydroxide are added, and the pH value is tested and adjusted to 13. According to the copper plating loading ratio of 3 square decimeters per liter and the copper plating temperature of 41°C, continuous stirring and circulating filtration are carried out during the copper plating process to keep the plating solution transparent and free of impurities. After the copper plating is completed, the lens is cleaned with ultrasound.

[0076] The first copper plating agent is HSECu-801 copper plating solution, and the second copper plating agent is Cu800 copper plating supplement.

[0077] Among them, the S3 adopts the electroplating silver process when silver plating, and the parameters of the electroplating silver are: the electroplating silver water is: main salt silver nitrate 16g / L, potassium silver cyanide 112g / L, complexing agent ammonium acetate 121g / L, potassium hydroxide 70mL / L, brightener 15mL / L, electroplating parameters are pH10, temperature 36°C, current 31A, specific gravity 22, time 50min, and ES-02A brightener is added during silver plating.

[0078] Wherein, the S3 is subjected to a galvanizing operation before silver plating, and the process parameters of the galvanizing operation are: using EN-AL-216 zinc immersion solution, the concentration is 260ml / L, the temperature is 27°C, the time is 15S, and the degree of beauty is 15Be.

[0079] Among them, when the S5 is solidified, deionization is used for cleaning when cleaning the silver-plated layer, and it is dried at 50-60°C; when passivating the silver-plated layer, it is treated with a dichromate solution to form a silver oxide and silver chromate film on the surface; when dipping the organic film, TX is coated on the surface of the silver layer to produce a complex protective film on the surface of the silver layer.

[0080] Among them, when the S6 is mirror-coated with back paint, electrostatic spraying of UV paint is adopted, the electrostatic pressure is controlled at 60-90KV, the flow rate pressure is set at 0.4MPa, the atomization pressure is set at 0.12MPa, the nozzle is 250mm away from the workpiece, the nozzle diameter is 16mm, and UV curing operation is performed after electrostatic spraying.

[0081] Among them, the S8 adopts a sampling inspection method during the mirror inspection, and the inspection parameters include: moisture and heat resistance, neutral salt spray resistance, optical properties, thickness, dimensional tolerance, diagonal difference and appearance quality.

[0082] Wherein, after the coating is found unqualified in the inspection, S8 uses nitric acid with a volume ratio of more than 50% to soak until the coating is completely removed, and then the coating operation is repeated.

[0083] Among them, the production process of the present invention is simple, the process is short, and the production cost is low; the silver mirror produced by the present invention has high reflectivity, and the reflectivity of the silver mirror is as high as more than 99%; the present invention also has a low dispersion characteristic, and the dispersion coefficient of the silver mirror is very low, only about one tenth of that of an ordinary glass lens, which can effectively avoid the chromatic aberration caused by the different refractive indices of light of different wavelengths, and provide a more realistic visual effect; in addition, the surface of the silver mirror of the present invention has strong corrosion resistance, and the silver film and back paint on the surface of the silver mirror have good corrosion resistance, which can maintain the reflectivity and clarity of the lens for a long time and extend the service life of the lens; in addition, the production process of the present invention is more environmentally friendly, and no harmful substances are used in the production process of the silver mirror, which meets environmental protection requirements.

[0084] In order to verify the superiority of the silver mirror of the present invention, the following experiments were conducted. During the experiments, the silver mirror produced by the comparative document 1 was selected as the control group, and the silver mirror produced by the embodiments 1 / 2 / 3 was selected as the experimental group. The following experiments were conducted respectively, and the experimental standards were as follows:

[0085] Shear strength: The shear strength between the coating and the coating and between the coating and the glass should be no less than 15N / cm2;

[0086] Moisture and heat resistance: After the moisture and heat resistance test, the reflective coating of the sample should not show any obvious changes, and the protective coating should not have bubbling or separation;

[0087] Neutral salt spray resistance: After the neutral salt spray test, the reflective layer of the sample is allowed to have 4 changes in diameter d<0.3m and 2 protective coating change points with a diameter d<2.5mm. The maximum inward extension of the edge coating loss is no more than 3.5mm.

[0088] Optical properties: The visible light reflectivity of silver mirrors should be no less than 85%. For colored silver mirrors, the visible light reflectivity should be no less than 75%;

[0089] In addition, the copper layer in Examples 1 / 2 / 3 of the present invention was tested. The copper layer is a bottom layer deposited on the substrate through a chemical process. The copper content in the copper layer should be no less than 200 mg / m2, and the test meets the standard.

[0090] The silver layer in Examples 1 / 2 / 3 of the present invention was tested. The silver layer had uniform reflective properties for visible light. The silver content in the silver layer should be no less than 700 mg / m2, and the test showed that the standard was met.

[0091] By converting the experimental data into percentages based on comparative file 1, the following table is obtained:

[0092] The generation process in the comparative document 1 is operated according to the embodiment disclosed therein, wherein the control of the relevant parameters is as follows: the pre-washed tempered glass substrate is baked to above 110°C for 10 minutes by using a 10% cerium oxide suspension before spraying the epoxy resin coating; the epoxy resin coating is sprayed and then continued to be baked at a temperature of 110°C for 15 minutes; the glass is left to stand at low temperature after silver plating and before passivation, and the low temperature standing is to keep the glass still in a space at a temperature of -5°C for 20 minutes, and the passivation process is performed after the glass returns to room temperature after the low temperature standing; the temperature of the first silver plating is 20°C, the silver plating time is 2 minutes, and the silver weight per unit area on the glass is 200 mg / m2; the temperature of the second silver plating is 30°C, the silver plating time is 1 minute, and the silver weight per unit area on the glass is 700 mg / m2. After the parameters of the comparative document 1 are tested as described above, the experimental results are statistically compared with the embodiments of the present invention, and the experimental results are percentage-based according to the experimental results of the comparative document 1, and the following experimental results are obtained:

[0093]

[0094] Through the above experiments, we can find that:

[0095] The various performances of Examples 1 / 2 / 3 of the present invention are more excellent than those of the comparative documents, indicating that the present invention has outstanding substantial features and significant progress.

[0096] By converting the experimental data into percentages based on comparative file 2, the following table is obtained:

[0097] Among them, the generation process in the comparative document 2 is operated according to the embodiment 1 disclosed therein, and the embodiment 1 of the comparative document 2 discloses its specific parameter settings in detail; after the parameters of the comparative document 2 are experimented according to the above, the experimental results are statistically compared with the embodiments of the present invention, and the experimental results are percentage-based according to the experimental results of the comparative document 2, and the following experimental results are obtained:

[0098]

[0099] It can be seen from the above experimental results that the experimental results of Example 1, Example 2 and Example 3 are improved in various related performances compared with the control group 1 and the control group 2.

[0100] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A production process for a silver mirror, characterized in that: The following steps are involved: S1. Raw material preparation: The raw materials prepared include pure silver and glass. Pure silver is made into silver plates through casting and other processes, and glass is made into lenses through cleaning, cutting and edge grinding processes; S2, chemical copper plating: chemical copper plating is performed on the surface of the lens; S3, Silver plating: Form a layer of silver film on the surface of the lens; S4, annealing: putting the silver-plated lens into a high-temperature furnace for annealing to eliminate the stress on the lens surface; S5, curing: including cleaning the silver-plated layer, passivating the silver-plated layer and dipping the organic film; S6, mirror coating back paint: spray back paint on the back of the lens; S7, mirror edge grinding: the annealed lens is edged to make the edge of the lens flat and smooth; S8. Mirror cleaning and inspection: Clean and inspect the edged lenses to ensure that the lens surface is clean, free of defects and meets quality standards.

2. The production process of a silver mirror according to claim 1, characterized in that: In the S2, a first copper precipitate and a second copper precipitate are selected for standby use, and the first copper precipitate, the second copper precipitate and deionized water are mixed in a mass ratio of 1:1:2, and then the lens is degreased and activated by pickling for 3 minutes. During the copper plating process, the first copper precipitate and sodium hydroxide are added, and the pH value is tested and adjusted to 12-13. According to the copper plating loading ratio of 2-4 square decimeters per liter, the copper plating temperature is 30-45°C, and continuous stirring and circulating filtration are carried out during the copper plating process to keep the plating solution transparent and free of impurities. After the copper plating is completed, the lens is cleaned with ultrasound.

3. The production process of a silver mirror according to claim 2, characterized in that: The first copper plating agent is copper plating solution HSECu-801, and the second copper plating agent is Cu800 copper plating supplement.

4. The production process of a silver mirror according to claim 1, characterized in that: When S3 is silver-plated, the electroplating silver process is adopted, and the parameters of the electroplating silver are: the electroplating silver water is: main salt silver nitrate 5-30g / L, potassium silver cyanide 80-130g / L, complexing agent ammonium acetate 80-130g / L, potassium hydroxide 40-90mL / L, brightener 5-20mL / L, electroplating parameters are pH 9-10, temperature 30-40°C, current 20-40A, specific gravity 20-25, time 40-60min, and ES-02A brightener is added during silver plating.

5. The production process of a silver mirror according to claim 1, characterized in that: Before silver plating, the S3 is subjected to a zinc plating operation, and the process parameters of the zinc plating operation are: using EN-AL-216 zinc immersion solution, the concentration is 200-300ml / L, the temperature is 20-40°C, the time is 10-20S, and the degree of beauty is 14-16Be.

6. The production process of a silver mirror according to claim 1, characterized in that: When the S5 is solidified, the silver-plated layer is cleaned by deionization and dried at 50-60° C.; when the silver-plated layer is passivated, it is treated with a dichromate solution to form a silver oxide and silver chromate film on the surface; when the organic film is immersed, one of TX, TF, SN, and LP-98S organic substances is coated on the surface of the silver layer to produce a complex protective film on the surface of the silver layer.

7. The production process of a silver mirror according to claim 1, characterized in that: When the S6 is mirror-coated with back paint, electrostatic spraying of UV paint is adopted, the electrostatic pressure is controlled at 60-90KV, the flow rate pressure is set at 0.3-0.5MPa, the atomization pressure is set at 0.05-0.15MPa, the nozzle is 200-300mm away from the workpiece, the nozzle diameter is 14-18mm, and UV curing operation is performed after electrostatic spraying.

8. The production process of a silver mirror according to claim 1, characterized in that: The S8 adopts a sampling inspection method when inspecting the mirror surface, and the inspection parameters include: moisture and heat resistance, neutral salt spray resistance, optical properties, thickness, dimensional tolerance, diagonal difference and appearance quality.

9. The production process of a silver mirror according to claim 1, characterized in that: After the S8 detects that the coating is unqualified, it uses nitric acid with a volume ratio of more than 50% to soak until the coating is completely removed, and then re-plating operation.