Low-water-consumption low-temperature-rise high-impermeability concrete and preparation method thereof

By optimizing the preparation of sand and gravel aggregates and fly ash, combined with water reducing agents and gas induction agents, the water consumption and temperature rise problems of concrete are solved, the mechanical properties and durability of concrete are improved, and it is suitable for large-volume and underground structures.

CN118878271APending Publication Date: 2024-11-01BEIJING GAOQIANG CONCRETE +2
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410811294.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

When existing concrete reduces water consumption, it ignores the temperature rise and heat shrinkage properties, resulting in durability and structural stability issues, and the mechanical performance evaluation is deviated from the actual engineering temperature environment.

Method used

By optimizing the crushing process and particle preparation of sand and gravel aggregates, low water consumption fly ash and dolomite powder are used, combined with polycarboxylic acid water reducing agent and gas induction agent, a low-temperature rise concrete mix ratio is designed to reduce the water of concrete Temperature rise and shrinkage performance improves the mechanical properties and durability of concrete.

Benefits of technology

Achieve high-seepage concrete with low water consumption and low temperature rise, significantly reduces the water consumption and temperature rise of concrete, improves the volume stability and durability of concrete, and reduces the risk of temperature rise cracks. It is suitable for large volumes and underground structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004906238460000051
    Figure BDA0004906238460000051
  • Figure BDA0004906238460000071
    Figure BDA0004906238460000071
  • Figure BDA0004906238460000081
    Figure BDA0004906238460000081
Patent Text Reader

Abstract

The invention relates to the technical field of concrete, and particularly discloses high-impermeability concrete with low water consumption and low temperature rise and a preparation method of the high-impermeability concrete. The concrete disclosed by the invention is prepared from the following components in parts by weight: 120 to 135 parts of water, 140 to 160 parts of cement, 125 to 145 parts of grade I fly ash, 43 to 58 parts of grade II dolomite powder, 845 to 865 parts of machine-made sand, 965 to 990 parts of gravel, 4.0 to 4.8 parts of polycarboxylate superplasticizer, 0.4 to 0.6 part of air entraining agent and 0.02 to 0.04 part of viscosity improver, the broken stones are formed by mixing broken stones of 5-10 mm and broken stones of 10-20 mm according to the weight ratio of (2-4): (6-8). The concrete prepared by using the technical scheme provided by the invention can effectively reduce the water consumption, improve the performance of the concrete, reduce temperature cracks caused by temperature rise of the concrete and improve the durability of the concrete.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of concrete, and in particular to a high-impermeability concrete with low water consumption and low temperature rise and a preparation method thereof. Background Art

[0002] The slump of concrete increases with the increase of water consumption, while the strength decreases with the increase of water consumption. That is, reducing water consumption can improve the strength and durability of concrete. At present, the water consumption of concrete is usually reduced by optimizing raw materials, using the water-reducing effect of high-efficiency water-reducing agents with high water-reducing rates, and reducing the porosity by multi-grading of sand and gravel aggregates.

[0003] In addition, when evaluating the durability of low-water-consumption concrete, there is a neglect of the thermal shrinkage performance caused by the temperature rise of concrete. At the same time, there is a misunderstanding that the evaluation of the mechanical properties of concrete is separated from the temperature environment of the engineering structure entity and is simply conducted under standard curing conditions for indoor test evaluation to draw conclusions.

[0004] Therefore, a high-impermeability concrete with strong mechanical properties, low water consumption and low temperature rise is needed to solve these problems. Summary of the invention

[0005] In order to improve the mechanical properties of high-permeability concrete materials with low water consumption and low temperature rise, the present application provides high-permeability concrete with low water consumption and low temperature rise and a preparation method thereof.

[0006] The present application provides a high-impermeability concrete with low water consumption and low temperature rise, which specifically comprises the following components in parts by weight: 120-135 parts of water, 140-160 parts of cement, 125-145 parts of Class I fly ash, 43-58 parts of Class II dolomite powder, 845-865 parts of machine-made sand, 965-990 parts of crushed stone, 4.0-4.8 parts of polycarboxylate water reducer, 0.4-0.6 parts of air entraining agent, and 0.02-0.04 parts of viscosity improver; The porosity of the crushed stone is less than 40%, and the crushed stone is composed of 5-10 mm crushed stone and 10-20 mm crushed stone mixed in a weight ratio of 2-4:6-8.

[0007] The technical solution provided in this application first proposes to optimize the crushing process of sand and gravel aggregates, combine the jaw crusher method with the vertical cone crusher method to achieve secondary crushing, and cooperate with mining companies to transform the production line to produce aggregate particles with excellent particle shape close to the ideal octahedron model. Through grading adjustment and optimization, 5-10mm and 10-20mm crushed stones are used to prepare coarse aggregate secondary distribution crushed stones with a void ratio of <40% (the minimum void ratio is 38%) according to the secondary distribution method with the lowest void ratio, and the optimal ratio is 3:7. The various indicators of crushed stones are tested. According to the irregular particle test method in JG / T568-2019 "Aggregates for High-Performance Concrete", the irregular particle content is determined to be 4% using a bar sieve, and all indicators meet the special grade standards for crushed stones.

[0008] Through the secondary crushing and shaping process, the particle grading of the machine-made fine aggregate was analyzed, and the machine-made sand zone II medium sand with round particles and grading close to natural river sand was prepared. The specific indicators were stone powder content (MB value 0.8) less than 7%, and fineness modulus of 2.6; the particle roundness evaluation was based on the flaky particle test method in JG / T568-2019 "Aggregates for High Performance Concrete", and the flaky particles were determined to be 8% using a bar sieve. All indicators met the special standards for artificial sand.

[0009] The sand-gravel ratio was set according to the Fuller curve, and the initial design sand ratio was 40-43% and verified by experiments; the density was 2200kg / m 3 Class I F fly ash (water requirement ratio 93%, fineness 18% and ignition loss 2.1%) replaces the density of 3100kg / m 3 Ordinary Portland cement makes full use of the filling effect. In the concrete system with fixed sand and gravel porosity, the net paste volume of water and cementitious materials is also fixed. When the same weight of fly ash replaces cement, the net paste volume will increase by 50% of the original cement volume. Under the same fluidity conditions, the same volume of water can be reduced to achieve the physical water reduction effect. After experimental verification, the water consumption of concrete can be significantly reduced to 155kg / m by replacing the same weight of cement with 50% fly ash. 3 the following.

[0010] The secondary crushing and shaping of artificial sand and gravel can optimize the particle shape and grading. At the same time, a large amount of stone powder is generated in the process of removing edges and corners to optimize the particle shape. The stone powder is collected by dust collectors. According to statistics, the proportion of stone powder in sand is up to 40%. The filling effect of stone powder in cement cementitious system and its easy dispersion effect under the action of water reducing agent and surfactant can be fully utilized to reduce water consumption or admixture dosage, which can also solve the problem of full resource utilization of shaped sand and gravel.

[0011] The filling effect of dust-collected dolomite powder produced during the crushing and shaping of artificial sand and gravel in the cement cementitious system and its easy dispersibility for water reducers are utilized to reduce the water consumption or the dosage of admixtures; the mix design method adopts the volume method design, which follows the design method of reducing the water consumption and reducing the cementitious materials in the same proportion under the premise of the same water-cement ratio, while increasing the proportion of sand and gravel aggregates, reducing the total amount of cementitious materials and the mortar-aggregate ratio, thereby reducing the hydration temperature rise of concrete and the shrinkage performance of concrete, improving the volume stability and density of concrete, and generally improving the durability of concrete.

[0012] The concrete mix design adopts the volumetric design method. Water, cementitious materials, admixtures and sand and gravel aggregates together constitute the volume of 1 cubic meter of concrete. By keeping the water-cement ratio (the ratio of water to cementitious materials, an important parameter of concrete mix) unchanged, reducing the amount of water and reducing the cementitious materials in the same proportion, the amount of water and cementitious materials in the concrete are reduced, and the volume occupied is reduced. The amount of sand and gravel aggregate in 1 cubic meter of concrete is increased, and the slurry-aggregate ratio (the volume ratio of slurry composed of water and cementitious materials to aggregate) is greatly reduced. Water and cementitious materials undergo hydration reaction in concrete to generate hydration products, and the volume changes. Sand and gravel aggregates play the role of a skeleton in concrete and basically do not participate in the reaction, and their volume will not change significantly. Reducing the amount of cementitious materials, especially cement, can reduce the hydration temperature rise of concrete and reduce concrete shrinkage, thereby improving the volume stability of concrete and making it less likely to produce temperature rise cracks. The existence of cracks can cause external harmful media and moisture to penetrate into the surface of the steel bars along the cracks, causing durability problems such as steel corrosion and structural leakage, thereby affecting the overall durability of the concrete.

[0013] In concrete structures, high temperature rise can easily lead to temperature cracks. In these structures, actual temperature measurements have found that after concrete hydration, there is an obvious temperature rise, forming a temperature peak and a temperature curve that gently decreases. Depending on the structure size and heat dissipation conditions, the temperature peak can reach 60°C or even 80°C. Temperature has a positive correlation with the strength development of concrete. Generally, the higher the temperature, the faster the strength development. However, in the concrete mix design, the concrete strength is usually designed under standard curing conditions (temperature 20±2°C, relative humidity>95%), ignoring the huge impact of temperature on strength, resulting in a serious disconnect between test data and engineering practice. In the concrete strength test, the test method of synchronous temperature curing is adopted, that is, a temperature sensor is buried in the concrete structure, the temperature change in the concrete structure is monitored online and synchronously transmitted to the temperature control computer system with a specially customized temperature curing box through the signal transmitter connected to the sensor through the Internet of Things technology; by synchronizing the temperature in the concrete structure with the temperature of the temperature curing box, the concrete specimens are subjected to temperature synchronous curing, and the synchronous concrete strength is obtained to evaluate the true strength of the concrete in the structure, eliminating concerns about the strength of large-volume concrete structures, avoiding the erroneous practice of increasing the cement dosage to increase the strength of concrete that is already redundant in strength, and giving full play to the temperature control and crack control advantages of high-permeability concrete with low water consumption and low temperature rise, and reducing the risk of cracking caused by excessive concrete temperature rise.

[0014] Preferably, the concrete specifically comprises the following components in parts by weight: 123-130 parts of water, 145-155 parts of cement, 130-140 parts of grade I fly ash, 45-55 parts of grade II dolomite powder, 850-860 parts of machine-made sand, 970-985 parts of crushed stone, 4.2-4.5 parts of polycarboxylate water reducer, 0.45-0.55 parts of air entraining agent, and 0.025-0.035 parts of viscosity improver.

[0015] Preferably, the crushed stone is composed of a mixture of 5-10 mm crushed stone and 10-20 mm crushed stone in a weight ratio of 2.5-3.5:6.5-7.5.

[0016] Preferably, the air entraining agent is selected from any one or more of triterpene saponin and sodium rosinate.

[0017] Preferably, the air-entraining agent is composed of a mixture of triterpenoid saponins, apple polyphenols and piceatannol in a weight ratio of 15:1-3:0.2-0.8.

[0018] Preferably, the viscosity improver is selected from any one or more of hydroxypropyl methylcellulose, starch dextrin, xanthan gum, and microbially fermented polysaccharide bio-gum. Preferably, the viscosity improver is composed of hydroxypropyl methylcellulose and microbially fermented polysaccharide bio-gum mixed in a weight ratio of 1-3:9.

[0019] Preferably, the viscosity of the hydroxypropyl methylcellulose is 4000-6500 mPa.s.

[0020] Preferably, the density of the Class I fly ash is 2100-2300 kg / m 3 , water requirement ratio 91-95%, fineness 17-19%, loss on ignition 2.0-2.2%.

[0021] The present application also provides a method for preparing the above-mentioned high-impermeability concrete with low water consumption and low temperature rise, which specifically comprises the following steps: According to weight, weigh the corresponding amount of each raw material component; Mix cement, Class I fly ash, Class II dolomite powder, machine-made sand and crushed stone to obtain dry material; Add polycarboxylate water reducer and viscosity improver into water, mix well, and obtain wet material; The dry material and the wet material are mixed evenly, and then an air entraining agent is added, stirred and mixed evenly, and the low water consumption and low temperature rise high impermeability concrete is obtained through vibration, molding and curing. In summary, the technical solution of this application has the following effects: The present application reduces the void ratio by utilizing high-quality aggregates that meet special grade indicators, thereby realizing a multi-graded low-void ratio sand and gravel aggregate combination; utilizes preferred fly ash and stone powder, adopts large-amount fly ash and stone powder technology, and composites high-performance water reducers, air entraining agents, and viscosity improvers, thereby reducing water consumption and improving concrete performance; reducing water consumption at the same water-cement ratio, reducing the amount of cementitious materials at the same ratio, increasing the aggregate volume content, reducing the mortar-to-aggregate ratio, and improving the volume stability of concrete, especially the thermal stability, are the keys to improving durability.

[0022] The concrete provided in this application is applied to the ready-mixed concrete industry, and has particularly good application prospects in concrete projects with high requirements for early temperature rise cracking, such as large-volume concrete, underground long wall anti-leakage projects, and water plant pool side walls. It can also be applied to ordinary concrete structures to reduce temperature cracks caused by concrete temperature rise, and can generally improve the durability of concrete. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a diagram showing the thermal insulation temperature rise performance of concrete in Example 3 and Comparative Example 1.

[0024] Figure 2 It is a diagram showing the thermal insulation temperature rise performance of concrete in Example 3 and Comparative Example 1.

[0025] Figure 3 The figure shows the drying shrinkage performance of the concrete in Example 3 and Comparative Example 1.

[0026] Figure 4The figure shows the autogenous shrinkage performance of concrete in Example 3 and Comparative Example 1.

[0027] Figure 5 The figure shows the frost resistance of concrete in Example 3 and Comparative Example 1.

[0028] Figure 6 The figure shows the chloride ion penetration resistance of concrete in Example 3 and Comparative Example 1.

[0029] Figure 7 It is a performance diagram of the analysis of the bubble spacing coefficient of the hardened concrete in Example 3 and Comparative Example 1. DETAILED DESCRIPTION

[0030] The raw materials used in this application, including triterpenoid saponin air-entraining agent extracted from plants, are sourced from Shanghai Fengyang Building Materials Co., Ltd.; apple polyphenols, piceatannol, green tea polyphenols, and farnesol are sourced from Mufan Biotechnology Co., Ltd.; microbial fermentation of polysaccharide bio-gum is sourced from Shijiazhuang Lanyan Building Materials Technology Co., Ltd.; hydroxypropyl methylcellulose is sourced from Shanghai Yuanye Biotechnology Co., Ltd.; the remaining raw materials and reagents can be obtained commercially.

[0031] The present application is further described in detail below in conjunction with examples, comparative examples and performance testing experiments. These examples should not be construed as limiting the scope of protection claimed in the present application. Example

[0032] Examples 1-3 Examples 1-3 respectively provide a high-permeability concrete with low water consumption and low temperature rise.

[0033] The difference between the above embodiments is that the amount of each raw material component in the high-permeability concrete with low water consumption and low temperature rise is different, as shown in Table 1.

[0034] The specific preparation process of the high impermeability concrete with low water consumption and low temperature rise in the above embodiment is as follows: According to the formula requirements shown in Table 1, weigh the corresponding weight portions of each raw material component; PO 42.5 ordinary Portland cement, Class I fly ash, Class II dolomite powder, machine-made sand, and crushed stone (the porosity of the crushed stone is 38%, and the crushed stone is 5-10 mm and 10-20 mm in a weight ratio of 3:7) are mixed evenly to obtain dry material; polycarboxylate water reducer and viscosity improver (hydroxypropyl methylcellulose with a viscosity of 4000-6500 mPa.s and polysaccharide bio-gum fermented by microorganisms are mixed in a weight ratio of 2:9) are added to water, mixed evenly, and wet material is obtained; The dry material and the wet material are mixed evenly, and then an air entraining agent (composed of a mixture of triterpenoid saponin, apple polyphenols and piceatannol in a weight ratio of 15:2:0.5) is added, and the mixture is stirred and mixed evenly. After vibration, molding and curing, the high impermeability concrete with low water consumption and low temperature rise is obtained.

[0035] Table 1 Amount of each raw material component in the high permeability concrete with low water consumption and low temperature rise in Examples 1-3 and Comparative Example 1 Embodiment 4-5 Examples 4-5 respectively provide a high-permeability concrete with low water consumption and low temperature rise.

[0036] The difference between the above embodiment and embodiment 3 is that the types of crushed stones in the high-impermeability concrete with low water consumption and low temperature rise are different, as shown below.

[0037] In Example 4, the crushed stone is composed of 5-10 mm crushed stone and 10-20 mm crushed stone mixed in a weight ratio of 2:8.

[0038] In Example 5, the crushed stones are composed of 5-10 mm crushed stones and 10-20 mm crushed stones mixed in a weight ratio of 4:6.

[0039] The remaining components, the amounts of the components, and the method for preparing the high-impermeability concrete with low water consumption and low temperature rise in the above embodiment are the same as those in embodiment 3.

[0040] Examples 6-12 Examples 6-12 respectively provide a high-permeability concrete with low water consumption and low temperature rise.

[0041] The difference between the above embodiment and embodiment 3 is that the types of air entraining agents are different, as shown below.

[0042] In Example 6, the air-entraining agent is composed of a mixture of sodium rosinate, apple polyphenols and piceatannol in a weight ratio of 15:2:0.5.

[0043] In Example 7, the air-entraining agent is composed of a mixture of triterpenoid saponins, green tea polyphenols and piceatannol in a weight ratio of 15:2:0.5.

[0044] In Example 8, the air-entraining agent is composed of a mixture of triterpenoid saponins, apple polyphenols and farnesol in a weight ratio of 15:2:0.5.

[0045] In Example 9: the air entraining agent is triterpene saponin.

[0046] In Example 10, the air-entraining agent is composed of a mixture of triterpenoid saponins, apple polyphenols and piceatannol in a weight ratio of 15:0.5:2.

[0047] In Example 11, the air-entraining agent is composed of a mixture of triterpenoid saponins, apple polyphenols and piceatannol in a weight ratio of 15:3:0.2.

[0048] In Example 12, the air-entraining agent is composed of a mixture of triterpenoid saponins, apple polyphenols and piceatannol in a weight ratio of 15:1:0.2.

[0049] The remaining components, the amounts of the components, and the method for preparing the high-impermeability concrete with low water consumption and low temperature rise in the above embodiment are the same as those in embodiment 3.

[0050] Examples 13-16 Examples 13-16 respectively provide a high-permeability concrete with low water consumption and low temperature rise.

[0051] The difference between the above embodiment and embodiment 3 is that the types of viscosity improvers in the high-impermeability concrete with low water consumption and low temperature rise are different, as shown below.

[0052] In Example 13: the viscosity improver is composed of hydroxypropyl methylcellulose and xanthan gum mixed in a weight ratio of 2:9.

[0053] In Example 14: the viscosity improver is composed of hydroxypropyl methylcellulose with a viscosity of 4000-6500 mPa.s and microbially fermented polysaccharide bio-gum mixed in a weight ratio of 5:9.

[0054] In Example 15: the viscosity improver is composed of hydroxypropyl methylcellulose (low viscosity, 400 mPa.s) and microbially fermented polysaccharide bio-gum mixed in a weight ratio of 2:9.

[0055] In Example 16: the viscosity improver is composed of hydroxypropyl methylcellulose (high viscosity, 30000 mPa.s) and microbially fermented polysaccharide bio-gum in a weight ratio of 2:9.

[0056] The remaining components, the amounts of the components, and the method for preparing the high-impermeability concrete with low water consumption and low temperature rise in the above embodiment are the same as those in embodiment 3.

[0057] Comparative Example Comparative Example 1 This comparative example provides a high impermeability concrete with low water consumption and low temperature rise.

[0058] The difference between this comparative example and Example 3 is that the dosage of each raw material component is different, as shown in Table 1.

[0059] The preparation method of the high impermeability concrete with low water consumption and low temperature rise in this comparative example is the same as that in Example 3.

[0060] Comparative Examples 2-4 Comparative Examples 2-4 respectively provide a high impermeability concrete with low water consumption and low temperature rise.

[0061] The difference between the comparative example and Example 3 is that the types of gravel are different, as shown below.

[0062] In Comparative Example 2: the crushed stone is 5-10 mm crushed stone.

[0063] In Example 3, the crushed stones are composed of 5-10 mm crushed stones and 10-20 mm crushed stones mixed in a weight ratio of 1:9.

[0064] In Comparative Example 4, the crushed stone is composed of 5-10 mm crushed stone and 10-20 mm crushed stone mixed in a weight ratio of 7:3.

[0065] The remaining components, the amounts of the components, and the method for preparing the high-impermeability concrete with low water consumption and low temperature rise in the above comparative example are the same as those in Example 3.

[0066] Performance testing (1) Concrete mixture properties and mechanical properties The performance and mechanical properties of concrete mixtures were tested in accordance with GB / T50080-2016 "Standard for Test Methods for Performance of Ordinary Concrete Mixtures" and GB / T50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Ordinary Concrete", and the yield stress and plastic viscosity indicators were determined using the Danish GERMANN ICAR concrete rheometer.

[0067] Test results: as shown in Table 2.

[0068] Table 2 Performance test results of high impermeability concrete with low water consumption and low temperature rise in Examples 1-16 and Comparative Examples 1-4 Combined with Table 2, by comparing the mixing performance and mechanical properties of the benchmark concrete in Example 3 with that in Comparative Example 1, it can be seen that the concrete in the optimized embodiment has similar slump and expansion to the benchmark concrete mixture, and the collapse and emptying time is shortened; from the analysis of the two parameters of the rheological properties of concrete, the yield shear stress τ0 and the plastic viscosity coefficient η of the optimized concrete show obvious changes, the yield shear stress characterizes the thixotropic property and fluidity, and the yield shear stress is reduced from 290.3Pa to 66.2Pa, indicating that the concrete mixture has better thixotropic property and is easier to vibrate and compact; due to the effect of adding the viscosity improver, a concrete with a small yield stress and a large plastic viscosity is obtained, and a concrete mixture that is easy to flow and has a large dynamic viscosity and is relatively stable is very beneficial. This phenomenon characterizes the characteristics of the concrete mixture being easy to flow, not easy to segregate, and having good cohesiveness. In addition, the concrete strength of the present application at 3d, 7d, 28d and 60d is lower than that of the benchmark concrete, but 60d can also meet the C40 concrete acceptance standard; the long-term strength at the later 180d continues to increase, even exceeding the benchmark concrete. Such concrete can meet the structural engineering application scenarios of 60-day acceptance.

[0069] By comparing the test results of Examples 3, 4-5 and Comparative Examples 2-4, the present application can improve the performance of concrete by selecting crushed stone composed of 5-10 mm crushed stone and 10-20 mm crushed stone mixed in a weight ratio of 2-4:6-8.

[0070] By comparing the test results of Examples 3, 6-12, the present application uses a mixture of triterpenoid saponins, apple polyphenols, and piceatannol in a weight ratio of 15:1-3:0.2-0.8 to form an air-entraining agent, which can further reduce the yield stress of concrete and increase the plastic viscosity.

[0071] By comparing the test results of Examples 3 and 13-16, the present application uses hydroxypropyl methylcellulose and microbially fermented polysaccharide bio-gum mixed in a weight ratio of 1-3:9 to form a viscosity improver, which can further reduce the yield stress of concrete and increase the plastic viscosity.

[0072] (2) Thermal insulation performance The thermal insulation temperature rise performance of the concrete in Example 3 and Comparative Example 1 was tested. The results are as follows: Figure 1 As shown, from the temperature rise curve, it can be seen that the hydration heat adiabatic temperature rise of the optimized concrete in Example 3 and the benchmark concrete in Comparative Example 1 tends to be flat after 50 hours, and the optimized concrete is 8-10°C lower than the benchmark concrete, and the adiabatic temperature rise reduction effect is obvious. The analysis is mainly due to the reduction in the amount of cementitious material, the more gentle hydration heat release, the lower peak value, and the smaller temperature rise shrinkage of the concrete.

[0073] (3) Drying shrinkage performance The drying shrinkage performance of concrete under dry curing environment was measured by attaching strain gauges on the surface of concrete specimens. The micro-strain acquisition instrument recorded the strain of the concrete specimens in real time every 30 seconds during the test. A curve was drawn based on the collected data. The drying shrinkage performance of concrete in Example 3 and Comparative Example 1 is shown in FIG. Figure 3 shown.

[0074] from Figure 3 It can be seen that 100,000 data points were collected in 35 days. The reference concrete in comparative example 1 maintained a microstrain of 450-500 at about 28 to 35 days; the optimized concrete in Example 3 maintained a microstrain of about 300 at about 28 to 35 days, with a microstrain difference of about 150. The low-water-consumption concrete has a small mortar-bone ratio and a reduced amount of cementitious materials, which significantly improves the drying shrinkage performance of the concrete and significantly increases the volume stability.

[0075] (4) Autogenous shrinkage performance The bellows autogenous shrinkage tester is mainly used to measure the autogenous shrinkage performance index of cement paste, mortar and concrete. Autogenous shrinkage refers to the condition that the cement paste is not dehydrated from the outside world. Due to the continued internal cement hydration, the free water in the capillary pores is insufficient, which makes the relative humidity inside the paste decrease spontaneously, causing the internal capillary tension to increase and form internal stress, resulting in paste shrinkage deformation. For ordinary concrete, autogenous shrinkage is much smaller than drying shrinkage, and mainly occurs inside the concrete before and after demolding. Unlike ordinary concrete, the autogenous shrinkage of high-performance concrete is almost equal to the drying shrinkage in the total shrinkage, or even greater than the drying shrinkage. Literature experiments show that when the water-cement ratio is 0.40, the autogenous shrinkage of concrete accounts for 40% of the total shrinkage; when the water-binder ratio is 0.17, the autogenous shrinkage of concrete accounts for 100% of the total shrinkage. The addition of high-strength grade cement, high cement content, and ultra-fine mineral powder will increase the autogenous shrinkage of concrete.

[0076] Reducing the amount of water, reducing the amount of cementitious materials at the same water-binder ratio, and reducing the mortar-binder ratio can usually reduce the autogenous shrinkage. The autogenous shrinkage properties of the two concretes were measured by experiments. The autogenous shrinkage properties of the concrete in Example 3 and Comparative Example 1 are as follows: Figure 4 As shown. Figure 4 It can be seen that the 7d autogenous shrinkage rate of the benchmark concrete is 900×10 -6 The optimized concrete shrinkage rate at 7 days is 400×10 -6 Left and right, the difference is 479×10 -6 Compared with the benchmark, the shrinkage rate is reduced by 50%, and the performance optimization effect is very significant.

[0077] (5) Antifreeze performance The frost resistance of the concrete in Example 3 and Comparative Example 1 is as follows: Figure 5 As shown. Figure 5It can be seen that no special air entrainment measures were taken for the two mix ratios of C40 concrete, and the air content of the concrete was about 3.5%. After the rapid freeze-thaw cycle F300 times, the two groups of concrete specimens did not reach the damage standard and met the F300 requirements. From the analysis of the specimen weight loss rate and relative static elastic modulus, the relative static elastic modulus of the two mix ratios is not much different; the weight loss rate of the optimized concrete is significantly lower than that of the benchmark concrete, but the absolute value of the difference between the two is not large, and the optimized mix ratio concrete has better performance.

[0078] (6) Chloride ion penetration resistance The chloride ion penetration resistance of concrete in Example 3 and Comparative Example 1 is as follows: Figure 6 As shown. Figure 6 It can be seen that the 56-day coulomb capacity test results of concrete show that with the same water-binder ratio, the water consumption decreases and the coulomb capacity shows a decreasing trend. The coulomb capacity of concrete with optimized mix ratio is reduced to 355C, which reaches QV level according to JGJ / T193-2009 "Concrete Durability Test and Evaluation Standard"; the coulomb capacity of the benchmark mix ratio is 647C, reaching Q-IV level.

[0079] (7) Analysis of air bubble spacing coefficient of hardened concrete The hardened concrete bubble spacing coefficient analysis performance of the concrete in Example 3 and Comparative Example 1 is as follows: Figure 7 As shown in Table 3. Figure 7 It can be seen that after the concrete specimens were sliced ​​and polished after curing for 28 days, and tested on the bubble spacing coefficient tester, the bubble spacing coefficient of the optimized concrete was 0.029mm, which was nearly an order of magnitude lower than the bubble spacing coefficient of the benchmark concrete of 0.212, showing a significant improvement. Through the analysis of the percentage of bubble area of ​​each particle size, it can be seen that the bubble distribution particle size in the optimized concrete is more uniform and has a wider distribution range, while the bubble distribution particle size range of the benchmark concrete is narrower and the distribution is more concentrated. The bubble spacing coefficient of concrete shows an increasing trend as the water consumption increases.

[0080] Table 3 Analysis results of concrete bubble spacing coefficient in Example 3 and Comparative Example 1 (8) Engineering Application A cable-stayed bridge across a river is designed with two super-large pedestals in the shape of a Chinese character "concave", with a height difference of 5.6 meters. The volume of a single pedestal is more than 4,500 cubic meters, which is a super-large concrete structure. The design requires that the pedestal structure should be C40 concrete, and the maximum temperature rise value should not exceed 55°C, and no temperature rise cracks should occur. In the construction of the project, low water consumption and low temperature rise technology is adopted, and 40% fly ash and 10% slag powder are added to replace 50% of the cement, reducing the cement content in the concrete to 202kg / m 3 , control the maximum temperature rise below 36℃ (temperature measurement curve as shown in Figure 7 There was no cracking in the concrete structure and the overall construction effect was good.

[0081] By testing and evaluating the thermal insulation temperature rise performance of the benchmark commonly used concrete in Comparative Example 1 and the optimized concrete after reducing the water consumption in Example 3, represented by C40, the thermal insulation temperature rise can be reduced by 8-10°C, and the thermal stability is significantly improved; construction practice has proved that the concrete performance of the optimized mix ratio has achieved excellent low water consumption and low temperature rise performance, and the early temperature rise cracking trend is significantly reduced.

[0082] Low-carbon concrete has developed rapidly in recent years. The main source of carbon emissions in the cement concrete industry is the cement manufacturing process, which produces an average of 0.6 tons of CO2 per ton of clinker. The low-water-consumption and low-temperature-rise concrete prepared by the technical solution of this application is mixed with a large amount of solid waste materials such as fly ash and dolomite powder, which significantly reduces the amount of cement used and has good durability, reducing the total amount of concrete within a fixed life cycle. It has obvious low-carbon concrete characteristics and is highly practical.

[0083] Although the present invention has been described in detail above with general descriptions and specific embodiments, it is obvious to those skilled in the art that some modifications or improvements may be made thereto based on the present invention. Therefore, these modifications or improvements made without departing from the spirit of the present invention all fall within the scope of protection claimed by the present invention.

Claims

1. A high impermeability concrete with low water consumption and low temperature rise, characterized in that: Specifically, it includes the following components in parts by weight: 120-135 parts of water, 140-160 parts of cement, 125-145 parts of Class I fly ash, 43-58 parts of Class II dolomite powder, 845-865 parts of machine-made sand, 965-990 parts of crushed stone, 4.0-4.8 parts of polycarboxylate water reducer, 0.4-0.6 parts of air entraining agent, and 0.02-0.04 parts of viscosity improver; The porosity of the crushed stone is less than 40%, and the crushed stone is composed of 5-10 mm crushed stone and 10-20 mm crushed stone mixed in a weight ratio of 2-4:6-8.

2. The high-impermeability concrete with low water consumption and low temperature rise according to claim 1, characterized in that: Specifically, it includes the following components in parts by weight: 123-130 parts of water, 145-155 parts of cement, 130-140 parts of Class I fly ash, 45-55 parts of Class II dolomite powder, 850-860 parts of machine-made sand, 970-985 parts of crushed stone, 4.2-4.5 parts of polycarboxylic acid water reducer, 0.45-0.55 parts of air entraining agent, and 0.025-0.035 parts of viscosity improver.

3. The high-impermeability concrete with low water consumption and low temperature rise according to claim 1, characterized in that: The crushed stones are composed of 5-10 mm crushed stones and 10-20 mm crushed stones mixed in a weight ratio of 2.5-3.5:6.5-7.

5.

4. The high impermeability concrete with low water consumption and low temperature rise according to claim 1, characterized in that: The air entraining agent is selected from any one or more of triterpenoid saponins and sodium rosinate.

5. The high impermeability concrete with low water consumption and low temperature rise according to claim 1, characterized in that: The air entraining agent is composed of a mixture of triterpenoid saponin, apple polyphenol and piceatannol in a weight ratio of 15:1-3:0.2-0.

8.

6. The high impermeability concrete with low water consumption and low temperature rise according to claim 1, characterized in that: The viscosity improver is selected from any one or more of hydroxypropyl methylcellulose, starch dextrin, xanthan gum, and polysaccharide bio-gum fermented by microorganisms.

7. The high impermeability concrete with low water consumption and low temperature rise according to claim 6, characterized in that: The viscosity improver is composed of hydroxypropyl methylcellulose and polysaccharide bio-gum fermented by microorganisms in a weight ratio of 1-3:

9.

8. The high impermeability concrete with low water consumption and low temperature rise according to claim 7, characterized in that: The viscosity of the hydroxypropyl methylcellulose is 4000-6500 mpa.s.

9. The high impermeability concrete with low water consumption and low temperature rise according to claim 1, characterized in that: The density of the Class I fly ash is 2100-2300 kg / m 3 , water requirement ratio 91-95%, fineness 17-19%, loss on ignition 2.0-2.2%.

10. The method for preparing high-impermeability concrete with low water consumption and low temperature rise according to any one of claims 1 to 9, characterized in that: The specific steps include: According to weight, weigh the corresponding amount of each raw material component; Mix cement, Class I fly ash, Class II dolomite powder, machine-made sand and crushed stone to obtain dry material; Add polycarboxylate water reducer and viscosity improver into water, mix well, and obtain wet material; The dry material and the wet material are mixed evenly, and then an air entraining agent is added, and the mixture is stirred and mixed evenly. After vibration, molding and curing, the high impermeability concrete with low water consumption and low temperature rise is obtained.

Citation Information

Patent Citations

  • Highly-impermeable C30 concrete with low rubber material consumption and preparation method thereof

    CN110041035A

  • Concrete doped with dolomitic rock powder, and preparation method thereof

    CN112745076A