Micro-expansion water purification sludge alkali-activated grouting material for backfilling urban waste underground pipelines and preparation method of micro-expansion water purification sludge alkali-activated grouting material

By using micro-expanded alkali-excited grouting materials prepared by using water-purified sludge, mineral powder and other materials, the problems of high backfill cost of urban waste underground pipelines and insufficient sludge treatment are solved, and environmentally friendly self-leveling filling and sludge resource utilization are achieved. The use of the pipe improves the compactness and compressive strength.

CN118878296AActive Publication Date: 2024-11-01XI'AN UNIVERSITY OF ARCHITECTURE AND TECHNOLOGY

Patent Information

Application Number
CN202411138212.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-01
Estimated Expiration
2044-08-19

AI Technical Summary

Technical Problem

The existing technology is costly and unenvironmental when dealing with backfill of urban abandoned underground pipelines, and the sludge treatment and disposal facilities are insufficient, making it difficult to effectively utilize water purification sludge, resulting in environmental pollution and safety hazards.

Method used

Use water purification sludge, mineral powder, fly ash, quartz sand, exciters and expansion agents to prepare micro-expanded alkali-excited grouting materials, destroy the flocculation structure through potassium sodium tartrate, and stimulate gelling by sodium hydroxide and dihydrate gypsum The reaction is to generate hydrated aluminum silicate and hydrated calcium silicate, increase the compactness and strength of the material, avoid the use of cement, and achieve self-leveling backfill.

Benefits of technology

It realizes the effective utilization of water purification sludge, reduces dependence on natural resources, reduces environmental damage, has good fluidity and condensation performance, can effectively fill waste pipes, improves the compactness and compressive strength of the pipes, and complies with environmental protection. Require.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118878296A_ABST
    Figure CN118878296A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of solid waste utilization, and discloses a micro-expansion water purification sludge alkali-activated grouting material for backfilling urban waste underground pipelines and a preparation method thereof, the micro-expansion water purification sludge alkali-activated grouting material comprises the following raw materials by mass: 67 parts of water purification sludge, 18-21 parts of mineral powder, 18-21 parts of fly ash, 16 parts of quartz sand, 4-7 parts of an activator, 0.1-0.3 part of sodium potassium tartrate tetrahydrate, 0.1-0.4 part of a coagulant, and 0.2-0.4 part of a water reducer. 0.4 to 0.7 part of an expanding agent; the exciting agent comprises sodium hydroxide and dihydrate gypsum, and the grouting material comprises the following components in parts by mass: 3.5-5 parts of dihydrate gypsum and 0.5-2 parts of sodium hydroxide. According to the invention, the water purification sludge generated by the urban water purification plant can be effectively utilized and is used as the underground pipeline backfill grouting material, so that the water purification sludge is recycled, the use of cement is avoided, and the method has the advantage of environmental protection.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of solid waste utilization, and in particular relates to a micro-expanded water purification sludge alkali-activated grouting material for backfilling urban abandoned underground pipelines and a preparation method thereof. Background Art

[0002] When urban water treatment plants produce drinking water that meets the requirements of daily life, they use coagulation, sedimentation, filtration and disinfection as the main steps for water treatment. Water treatment sludge is a harmless and high-water content soil formed by coagulation and sedimentation treatment in water plants. It mainly includes minerals such as SiO2 and Al2O3 that are similar to clay in composition.

[0003] In terms of technology, sludge treatment methods are constantly innovating and improving, including sludge concentration, mechanical dehydration, drying, incineration, composting and biological treatment. Some new technologies and processes, such as sludge pyrolysis and sludge carbonization, are also emerging, providing more options for the development of the sludge treatment industry. However, if it is not handled properly, it is easy to cause direct or potential pollution to the environment. Therefore, how to effectively treat these wastes to achieve the goals of harmlessness, reduction and resource utilization is a key issue in the current global environmental protection field.

[0004] At present, although the sludge treatment and disposal industry has developed rapidly, there are still some problems, such as insufficient sludge treatment and disposal facilities and the technical level needs to be improved. In the future, with the continuous promotion of environmental protection policies and the continuous advancement of technology, the sludge treatment and disposal industry is expected to develop further and achieve more efficient and environmentally friendly sludge treatment and resource utilization.

[0005] In addition, with the increase of urban population and the expansion of cities, the original underground pipelines cannot bear the current demand. The cost of expansion on the original basis is huge and affects the normal life of residents. Therefore, some areas have abandoned the original pipelines. However, the abandoned underground sewer pipes in the city will bring a series of hazards. These hazards not only affect the urban environment, but may also have a serious impact on residents' lives and public safety.

[0006] Wastewater, sewage and other harmful substances may remain in abandoned sewer pipes. If these substances are not properly handled, they may leak into the soil and pollute groundwater. Groundwater is one of the important sources of domestic water for urban residents. Once polluted, it will directly affect the safety of drinking water for residents. It may also leak or collapse due to aging, damage or blockage, causing ground collapse or road damage, posing a threat to public safety.

[0007] Therefore, it is necessary to effectively fill the abandoned underground pipes to solve the above problems. However, if the traditional grouting filling process is used, it will be costly and not in line with the low-carbon and environmental protection concept. If the flocculated sludge from the water treatment plant can be solidified and given good rheological properties so that it can be self-leveled and filled in the abandoned underground pipes, it can not only solve the above problems, but also solve the sludge disposal problem.

[0008] In summary, water purification sludge treatment is an important issue in the current environmental protection field. Its development status shows that the market scale is expanding, technological innovation is active, but it still needs to be improved. In the future, with the promotion of relevant policies and technological progress, the water purification sludge treatment industry is expected to achieve more efficient and environmentally friendly development.

[0009] The invention patents for the current application of pipeline filling material technology are as follows:

[0010] Chinese invention patent application CN113004006A provides a foamed lightweight soil for backfilling abandoned oil pipelines and a preparation method thereof. The invention discloses a foamed lightweight soil for backfilling abandoned oil pipelines, comprising the following raw materials in parts by weight: 0-400 parts of cement, 100-1000 parts of admixture, 200-500 parts of water, 0-10 parts of reinforcing agent, 0.1-2 parts of retarder and 0.3-2 parts of foaming agent; preparation method: (1) weighing each raw material; (2) mixing and stirring cement, admixture, water, reinforcing agent and retarder at a speed of 50-150r / min for 2-5min to obtain a composite slurry; (3) first foaming the foaming agent to obtain foamed foam, and then stirring and mixing with the composite slurry; (4) pouring on site or prefabricating in a factory to obtain. The product of the invention has high internal closed-cell rate, good thermal insulation and sound insulation performance, and filling self-compactness; it can be widely applied to admixtures, which not only solves the problem of solid waste utilization, but also reduces hydration and achieves the purpose of slow-setting casting.

[0011] Chinese invention patent application CN114409324A proposes a filling material for abandoned oil and gas pipelines, a preparation method thereof, and a grouting process. The invention discloses a filling material for abandoned oil and gas pipelines, a preparation method thereof, and a grouting process, which belongs to the field of petrochemical industry. The filling material for abandoned oil and gas pipelines includes the following components in parts by weight: 80-100 parts of silt, 5-15 parts of cement, 120-150 parts of water, 0.1-0.5 parts of retarder, and 5-15 parts of expansion agent. The filling material only uses a very low weight portion of cement and a large amount of silt, which has better environmental friendliness and lower cost. The filling material has the advantages of high fluidity and long initial setting time, can meet the long-distance grouting requirements, and is particularly suitable for long-distance oil and gas pipelines. After solidification, the filling material has good strength and solidity, can achieve permanent solidification, and achieve good stability.

[0012] Chinese invention patent application CN110304877A proposes a foamed lightweight soil material and a preparation method thereof for large-scale filling projects. The present invention discloses a foamed lightweight soil material and a preparation method thereof for large-scale filling projects, wherein the raw materials include: powder, water, foaming agent, stimulant, and admixture. The lightweight foamed soil prepared by the present invention can be added with a large amount of solid waste raw materials, which effectively improves the utilization rate of solid waste and reduces production costs. At the same time, it can effectively realize large-scale equipment pumping and long-distance pipeline transportation, and the construction speed is fast, which meets the construction application of large-scale filling projects. The product has good uprightness, does not require high-temperature maintenance, and natural maintenance can meet standard requirements. It has great social benefits and economic value of energy saving and environmental protection, and turning waste into treasure, and has excellent industrialization prospects.

[0013] Chinese invention patent application CN103979880A proposes a cement multi-compound mixture of pipeline engineering trench backfill materials and a preparation method. The invention relates to building materials, and specifically to a cement multi-compound mixture of pipeline engineering trench backfill materials and a preparation method. The mixture is mainly composed of a mixture of crushed construction waste and soil, and is supplemented with a small amount of cement, the cement accounts for 3%-10% of the total amount of the mixture, the soil accounts for 35%-45% of the total amount of the mixture, the plasticity index of the soil is 10-20, and the water added accounts for 10%-16% of the mixture. Since the mixture has good workability, this backfilling method will not leave dead corners at the pipe armpits, and can evenly and densely fill every corner, which is safe and reliable; compared with traditional construction processes, this construction process saves a lot of manpower and material resources, greatly shortens the construction period, and is very worthy of promotion; in terms of material composition, we use construction waste, turn these wastes into treasures, generate value again, and realize energy saving and green environmental protection production concepts.

[0014] Although the above patents have the above advantages, they also have many shortcomings, as shown in Table 1:

[0015] Table 1

[0016]

[0017]

[0018] In summary, these patent applications may have common shortcomings in environmental risk assessment, performance stability, practical application limitations, long-term performance evaluation, and technological innovation and originality. Summary of the invention

[0019] In order to solve the problems existing in the prior art, the purpose of the present invention is to provide a micro-expanded water purification sludge alkali-activated grouting material for backfilling urban abandoned underground pipelines and a preparation method thereof. The present invention can effectively utilize the water purification sludge produced by urban water purification plants and use it as a grouting material for backfilling underground pipelines, thereby realizing the reuse of water purification sludge and avoiding the use of cement, and having the advantage of environmental protection.

[0020] The technical solution adopted by the present invention is as follows:

[0021] A micro-expanded water purification sludge alkali-activated grouting material for backfilling urban abandoned underground pipelines, wherein the raw materials thereof include, by weight:

[0022] 67 parts of water purification sludge, 18-21 parts of mineral powder, 18-21 parts of fly ash, 16 parts of quartz sand, 4-7 parts of activator, 0.1-0.3 parts of potassium sodium tartrate, 0.1-0.4 parts of coagulant, 0.2-0.4 parts of water reducer, 0.4-0.7 parts of expansion agent;

[0023] The activator comprises sodium hydroxide and dihydrate gypsum. Calculated by weight, the alkali-activated grouting material for backfilling micro-expanded water purification sludge in abandoned urban underground pipelines contains 3.5-5 parts of dihydrate gypsum and 0.5-2 parts of sodium hydroxide.

[0024] Preferably, in terms of mass percentage, the solid components of the water purification sludge contain: 87% to 94% SiO2, 6% to 12% Al2O3, and the remainder is other impurities. The water content of the water purification sludge can reach up to 260%.

[0025] Preferably, the mineral powder is S95 grade slag powder.

[0026] Preferably, the fly ash is primary fly ash.

[0027] Preferably, the quartz sand is ISO standard sand.

[0028] Preferably, the sodium hydroxide is of industrial grade above 99%, and the dihydrate gypsum is of industrial grade above 99%.

[0029] Preferably, the coagulant is anhydrous sodium sulfate.

[0030] Preferably, the water reducer is a naphthalene-based water reducer.

[0031] Preferably, the expansion agent is UEA expansion agent.

[0032] The present invention as described above is characterized in that the micro-expanded water purification sludge alkali-activated grouting material for backfilling urban abandoned underground pipelines comprises:

[0033] The water purification sludge and potassium sodium tartrate are uniformly mixed to obtain a mixture A;

[0034] Add mineral powder, fly ash, dihydrate gypsum and quartz sand into mixture A and stir evenly to obtain a mixed slurry;

[0035] Sodium hydroxide, a water reducing agent, an expansion agent and a coagulant are added into the mixed slurry and stirred evenly to obtain the micro-expansion water purification sludge alkali-activated grouting material for backfilling urban abandoned underground pipelines.

[0036] The present invention has the following beneficial effects:

[0037] In the micro-expansion alkali-activated grouting material based on water purification sludge of the present invention, a flocculant is added, and the flocculant includes potassium sodium tartrate (NaKC4H4O6), wherein the sodium ions generated by the hydrolysis of potassium sodium tartrate replace the aluminum ions in the water purification sludge, and the aluminum ions form a compatible complex by chelating with tartaric acid anions, thereby destroying the cellular structure of the flocculated water purification sludge, so that the water purification sludge has a higher fluidity in less water, and the mineral powder, fly ash and activator can coagulate and solidify the sludge, and sodium hydroxide and dihydrate gypsum are used as activators, and the increased OH - The concentration helps to break the Si-O and Al-O bonds in the fly ash particles, and the Ca 2 + Gelation reaction occurs to generate gel substances such as hydrated aluminum silicate and hydrated calcium silicate. Secondly, dihydrate gypsum, as a sulfate activator, can form new gelling substances with mineral admixtures to fill pores and enhance the density and strength of the material. Sulfate activators can also accelerate the coagulation and hardening process of mineral admixtures, improve early strength and have better durability and impermeability. The alkaline substances in the expansion agent react with calcium hydroxide in the mineral powder to generate a large amount of hydrated calcium aluminate (C2S) and hydrated calcium ferrate (C3A). The silicate minerals in the expansion agent decompose at high temperatures and release gas, which further aggravates the volume expansion and makes the inside of the pipe more substantial. Accelerate the hydration process to increase strength without affecting its flow properties. The initial fluidity of the mixed slurry should be 290mm, and the loss after 30min should be no less than 260mm, which is the basic process requirements of grouting materials, and the 28d strength should be above 1.5MPa. It can be seen that the present invention can effectively utilize the water purification sludge produced by the urban water purification plant and use it as a grouting material for backfilling underground pipelines, thereby realizing the reuse of the water purification sludge and avoiding the use of cement, thereby having the advantage of being environmentally friendly.

[0038] In the preparation method of the present invention, the prepared deflocculant is firstly put into the flocculated sludge and stirred to destroy the cellular structure and release free water, and then the mineral admixture is added and further stirred and mixed until it is uniform, and finally the stimulator and the admixture are added to achieve the solidification effect, thereby obtaining a slurry with good flowability and coagulation properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 The present invention is a flow chart for preparing the micro-expanded water purification sludge alkali-activated grouting material used for backfilling urban abandoned underground pipelines. DETAILED DESCRIPTION

[0040] The technical solution of the present invention is described below in conjunction with specific implementation examples. Each embodiment is an experimental example and provides real performance test data. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention.

[0041] The invention discloses a micro-expanded water purification sludge alkali-activated grouting material for backfilling abandoned underground pipes in cities. The raw materials thereof include, by weight, 67 parts of water purification sludge, 18 to 21 parts of mineral powder, 18 to 21 parts of fly ash, 16 parts of quartz sand, 4 to 7 parts of activator, 0.1 to 0.4 parts of potassium sodium tartrate, 0.1 to 0.4 parts of coagulant, 0.2 to 0.4 parts of water reducer and 0.4 to 0.7 parts of expander. The activator includes sodium hydroxide and dihydrate gypsum. By weight, the micro-expanded water purification sludge alkali-activated grouting material for backfilling abandoned underground pipes in cities contains 3.5 to 5 parts of dihydrate gypsum and 0.5 to 2 parts of sodium hydroxide.

[0042] Among them, the fly ash adopts first-grade fly ash. The quartz sand adopts ISO standard sand. The dihydrate gypsum adopts industrial grade above 99%. The mineral powder adopts S95 grade slag powder. The water reducer adopts naphthalene water reducer, and the effective amount is ≥94%. The alkali sodium hydroxide adopts industrial grade above 99%. The potassium sodium tartrate adopts industrial grade above 99%. The coagulant adopts anhydrous sodium sulfate of industrial grade above 99%. The UEA expansion agent is industrial grade above 99%.

[0043] Reference Figure 1 The present invention provides a method for preparing a micro-expanded water purification sludge alkali-activated grouting material for backfilling urban abandoned underground pipelines, comprising the following steps:

[0044] Weigh fly ash, mineral powder, dihydrate gypsum, sodium hydroxide, water purification sludge, flocculant potassium sodium tartrate, quartz sand, expansion agent, water reducing agent and coagulant according to the proportion;

[0045] Pour the water purification sludge and flocculant into the NJ-160A mixer and mix them. The mixer has a low revolution speed of 65r / min and stirs for 240 seconds to mix them evenly.

[0046] Then, fly ash, mineral powder, dihydrate gypsum and quartz sand are put into a mixer, the revolution speed of the mixer is a low speed of 65r / min, and the mixture is stirred for 120 seconds to obtain a mixed slurry;

[0047] Then, sodium hydroxide, water reducing agent, expansion agent and coagulant are poured into a mixer, the mixer revolution speed is high speed 130r / min, stirring for 120 seconds, and mixing evenly to obtain the micro-expansion water purification sludge alkali-activated grouting material for backfilling urban abandoned underground pipelines of the present invention.

[0048] The specific mechanism of the technical solution of the present invention is explained as follows:

[0049] In the technical solution of the present invention, with the addition of potassium sodium tartrate (NaKC4H4O6), the sodium ions hydrolyzed from potassium sodium tartrate replace aluminum ions through ion exchange, so that the replaced aluminum ions are synthesized into a compatible complex with tartrate ions to supplement the steric hindrance effect, so that the water purification sludge has higher fluidity in less water and is evenly dispersed. The ions generated after the hydrolysis of potassium sodium tartrate hydrolyze PAC (polyaluminium chloride), and then the coagulated and flocculated aluminium ions are replaced to form new soluble substances, which destroy the colloidal structure of aluminium hydroxide generated by the hydrolysis of the original aluminium ions and release the enclosed free water. Then mineral admixtures and stimulants are added. The mineral admixtures and stimulants act to coagulate and solidify the sludge. However, under the influence of high sludge moisture content, residual flocculants and the slowing effect of potassium sodium tartrate on the activation of mineral admixtures by the stimulant, the coagulation and hardening time of the slurry is severely weakened. It can only be formed in three days, but it still cannot coagulate. Therefore, the accelerating component - anhydrous sodium sulfate is added to accelerate the hydration process and improve the strength. In addition, the sulfate introduced by the alkali-free quick-setting agent can also stimulate the admixture, [Al(OH)4] - and SO4 2- A large amount of ettringite (AFt) is generated in the liquid phase to fill the pores caused by the high water content, thereby increasing the strength. The later 28d compressive strength is also not affected. However, it does not affect its flowability, which meets the basic process requirements of grouting materials.

[0050] The activators are sodium hydroxide and gypsum. First, as a strong alkaline substance, sodium hydroxide can increase the OH content in the slurry during the activation process. - This increase in OH - The concentration helps to break the Si-O and Al-O bonds in the fly ash particles, thereby forming a large number of free unsaturated active bonds on the surface of the fly ash particles. These unsaturated active bonds react with Ca in the solution in an alkaline environment. 2+ A gelling reaction occurs to generate gel substances such as hydrated aluminum silicate and hydrated calcium silicate. Secondly, for mineral admixtures, the role of sodium hydroxide excitation is mainly to activate the potential active ingredients therein. Mineral admixtures, such as fly ash, although rich in inorganic components, have been studied and their own activity is not sufficient to fully exert their improvement effect in concrete. The present invention is stimulated by sodium hydroxide, so that the active ingredients in the mineral admixtures are more fully released and reacted, thereby chemically reacting with the calcium hydroxide component in the mineral powder to generate more gelling substances. In addition, with the continuous accumulation of gelling substances, its principle is similar to the snowball effect, and it will eventually combine with the Al element in the additive and free water to undergo a hardening reaction to generate substances with higher strength such as ettringite. Secondly, gypsum, as a sulfate activator, can react chemically with active ingredients such as aluminum oxide and silicon oxide in mineral admixtures to form new gelling substances, such as ettringite and hydrated calcium silicate (CSH gel). These newly formed substances can fill pores and enhance the density and strength of the material. Sulfate activators can also accelerate the setting and hardening process of mineral admixtures and improve early strength. Mineral admixtures activated by sulfates usually have better durability and impermeability. This is because the newly formed gelling substances can block the pores and reduce the penetration of moisture and harmful ions. The alkaline substances in the expander react with the calcium hydroxide in the mineral powder to produce a large amount of hydrated calcium aluminate (C2S) and hydrated calcium ferrate (C3A). These newly formed compounds will continue to hydrolyze in the later stage, producing a large amount of water vapor, resulting in volume expansion. Decomposition of silicate minerals: The silicate minerals in the expander decompose at high temperatures and release gases, which further aggravates the volume expansion and makes the inside of the pipe more substantial.

[0051] In summary, the use of water purification sludge and stimulated mineral admixtures in the present invention can not only reduce dependence on natural resources and reduce environmental damage, but also, since mineral admixtures are usually industrial byproducts, their use can also help realize the resource utilization of waste.

[0052] The following is further explained in conjunction with specific embodiments. The water purification sludge used in the following embodiments of the present invention is water purification sludge produced by a tap water treatment plant. Calculated by mass percentage, the solid component of the water purification sludge contains: 93% SiO2, 6.5% Al2O3, and the remainder is other impurities; the water content of the water purification sludge is 260%.

[0053] Embodiment 1:

[0054] The present embodiment is used for the micro-expanding clean water sludge alkali-activated grouting material for backfilling urban abandoned underground pipelines. The raw materials include, by weight: 67 parts of clean water sludge, 18 parts of mineral powder, 18 parts of fly ash, 16 parts of quartz sand, 3.5 parts of dihydrate gypsum, 0.5 parts of sodium hydroxide, 0.1 parts of potassium sodium tartrate, 0.1 parts of anhydrous sodium sulfate, 0.2 parts of naphthalene-based water reducer, and 0.4 parts of UEA expansion agent.

[0055] The micro-expanded water purification sludge alkali-activated grouting material used for backfilling urban abandoned underground pipelines in this embodiment is prepared according to the above-mentioned preparation method.

[0056] Embodiment 2:

[0057] The present embodiment is used for the micro-expanding clean water sludge alkali-activated grouting material for backfilling urban abandoned underground pipelines. The raw materials include, by weight: 67 parts of clean water sludge, 18 parts of mineral powder, 18 parts of fly ash, 16 parts of quartz sand, 4.0 parts of dihydrate gypsum, 1.0 part of sodium hydroxide, 0.2 parts of potassium sodium tartrate, 0.2 parts of anhydrous sodium sulfate, 0.3 parts of naphthalene-based water reducer, and 0.5 parts of UEA expansion agent.

[0058] The micro-expanded water purification sludge alkali-activated grouting material used for backfilling urban abandoned underground pipelines in this embodiment is prepared according to the above-mentioned preparation method.

[0059] Embodiment 3:

[0060] The present embodiment is used for the micro-expanding clean water sludge alkali-activated grouting material for backfilling urban abandoned underground pipelines. The raw materials include, by weight: 67 parts of clean water sludge, 20 parts of mineral powder, 20 parts of fly ash, 16 parts of quartz sand, 4.5 parts of dihydrate gypsum, 1.5 parts of sodium hydroxide, 0.3 parts of potassium sodium tartrate, 0.3 parts of anhydrous sodium sulfate, 0.4 parts of naphthalene-based water reducer, and 0.6 parts of UEA expansion agent.

[0061] The micro-expanded water purification sludge alkali-activated grouting material used for backfilling urban abandoned underground pipelines in this embodiment is prepared according to the above-mentioned preparation method.

[0062] Embodiment 4:

[0063] The present embodiment is used for the micro-expanding clean water sludge alkali-activated grouting material for backfilling urban abandoned underground pipelines. The raw materials include, by weight: 67 parts of clean water sludge, 21 parts of mineral powder, 21 parts of fly ash, 16 parts of quartz sand, 5.0 parts of dihydrate gypsum, 2.0 parts of sodium hydroxide, 0.4 parts of potassium sodium tartrate, 0.4 parts of anhydrous sodium sulfate, 0.5 parts of naphthalene-based water reducer, and 0.7 parts of UEA expansion agent.

[0064] The micro-expanded water purification sludge alkali-activated grouting material used for backfilling urban abandoned underground pipelines in this embodiment is prepared according to the above-mentioned preparation method.

[0065] The grouting materials prepared in Examples 1 to 4 are tested for performance. The fluidity meets the requirements of the current national standard "Method for Determining Fluidity of Cement Mortar" GB / T2419. The initial fluidity ranges from 290 to 340 mm, the fluidity ranges from 270 to 310 mm after 30 min, and the density and expansion at 28 days are in accordance with the T0576-2020 cement concrete limited expansion rate test method. The compressive strength test shall be carried out in accordance with the relevant provisions of the current national standard "Test Method for Strength of Cement Mortar (ISO Method)" GB / T17671, and the range is 0.5 to 2.0 MPa. The specific test results are shown in Table 2 below:

[0066] Table 2

[0067]

[0068] It can be seen from the test results in Table 2 that in each embodiment, as the proportion of powder increases, the water-cement ratio of the slurry decreases relatively, and the fluidity decreases accordingly. The initial fluidity ranges from 290 to 340 mm, and the time loss ranges from 290 to 310 mm; the density increases accordingly with the increase of solid content, ranging from 0.80 to 0.90 / kg·m -3 ; As the proportion of cement increases, the amount of hydration products produced increases, and the compressive strength increases accordingly. The strength range is 0.5 to 1.8 MPa, which meets the fluidity and strength standards of grouting materials.

[0069] The porosity test was performed on the grouting materials prepared in the above-mentioned Examples 1 to 4, and the specific results are shown in Table 3 below:

[0070] Table 3

[0071]

[0072] It can be seen from the data in Table 3 that as the cement content increases, the solid content of the slurry also increases accordingly, and the expansion rate also decreases in the range of 0.5-0.8%, which meets the shrinkage standard of grouting materials.

[0073] It can be seen from the above scheme that the present invention aims at backfilling of abandoned underground pipes in cities, and proposes a scheme to achieve self-flowing and fully filling the pipe space by using a high-fluidity grouting material prepared by using water purification sludge, mineral admixtures, stimulants and additives. Compared with the previous resource utilization of water purification sludge, the preparation method of the present invention is simple, the required materials, water purification sludge and mineral admixtures, are all waste resources, which solves the disposal problem, and it has no toxic effects and has wide practicality.

Claims

1. A micro-expanded water purification sludge alkali-activated grouting material for backfilling urban abandoned underground pipelines, characterized in that: The raw materials include, by weight: 67 parts of water purification sludge, 18-21 parts of mineral powder, 18-21 parts of fly ash, 16 parts of quartz sand, 4-7 parts of activator, 0.1-0.4 parts of potassium sodium tartrate, 0.1-0.4 parts of coagulant, 0.2-0.4 parts of water reducer, 0.4-0.7 parts of expansion agent; The activator comprises sodium hydroxide and dihydrate gypsum. Calculated by weight, the alkali-activated grouting material for backfilling micro-expanded water purification sludge in abandoned urban underground pipelines contains 3.5-5 parts of dihydrate gypsum and 0.5-2 parts of sodium hydroxide.

2. The micro-expanded water purification sludge alkali-activated grouting material for backfilling urban abandoned underground pipelines according to claim 1, characterized in that: In terms of mass percentage, the solid components of the water purification sludge contain: 87% to 94% SiO2, 6% to 12% Al2O3, and the remainder is other impurities. The water content of the water purification sludge can reach up to 260%.

3. The micro-expanded water purification sludge alkali-activated grouting material for backfilling urban abandoned underground pipelines according to claim 1, characterized in that: The mineral powder is S95 grade slag powder.

4. The micro-expanded water purification sludge alkali-activated grouting material for backfilling urban abandoned underground pipelines according to claim 1, characterized in that: The fly ash is primary fly ash.

5. The micro-expanded water purification sludge alkali-activated grouting material for backfilling urban abandoned underground pipelines according to claim 1, characterized in that: The quartz sand is ISO standard sand.

6. The alkali-activated grouting material for backfilling micro-expanded water purification sludge in abandoned urban underground pipelines according to claim 1, characterized in that: The sodium hydroxide is of industrial grade above 99%, and the dihydrate gypsum is of industrial grade above 99%.

7. The alkali-activated grouting material for backfilling micro-expanded water purification sludge in abandoned urban underground pipelines according to claim 1, characterized in that: The coagulant is anhydrous sodium sulfate.

8. The alkali-activated grouting material for backfilling micro-expanded water purification sludge in abandoned urban underground pipelines according to claim 1, characterized in that: The water reducing agent is a naphthalene-based water reducing agent.

9. The alkali-activated grouting material for backfilling micro-expanded water purification sludge in abandoned urban underground pipelines according to claim 1, characterized in that: The expansion agent is UEA expansion agent.

10. The micro-expanded water purification sludge alkali-activated grouting material for backfilling urban abandoned underground pipelines according to any one of claims 1 to 9, characterized in that: include: The water purification sludge and potassium sodium tartrate are uniformly mixed to obtain a mixture A; Add mineral powder, fly ash, dihydrate gypsum and quartz sand into mixture A and stir evenly to obtain a mixed slurry; Sodium hydroxide, a water reducing agent, an expansion agent and a coagulant are added into the mixed slurry and stirred evenly to obtain the micro-expansion water purification sludge alkali-activated grouting material for backfilling urban abandoned underground pipelines.

Citation Information

Patent Citations

  • Pipeline engineering trench backfill material cement all-in-one mixture and preparation method thereof

    CN103979880A

  • Foam light soil material applied to large-scale filling projects, and preparation method thereof

    CN110304877A

  • Foamed light soil for backfilling waste petroleum pipelines and preparation method of foamed light soil

    CN113004006A

  • Filling material for waste oil and gas pipeline and preparation method and grouting process thereof

    CN114409324A

  • Method for preparing shield grouting liquid by utilizing waste mud

    CN107344830A

Cited By

  • Preparation method and application of self-leveling filling waste pipeline material

    CN120117855A

  • A method for preparing and applying a self-leveling filler for abandoned pipeline materials

    CN120117855B