Zirconium oxide grinding medium and preparation method thereof

Through the mixing and heat treatment of ultrafine 3YSZ powder, pure zirconia powder and nano yttrium oxide powder, the problem of low process difficulty and efficiency in the preparation of zirconia grinding media is solved, and a high purity and spherical zirconia grinding media is realized. Preparation, suitable for mass production.

CN118878320APending Publication Date: 2024-11-01JIANGXI GUOKE ZHONGLIAN NEW MATERIALS CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411101664.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

When preparing submillimeter-level spherical grinding media, the process technology is difficult, the production efficiency is low, and there is a contradiction between performance and efficiency of the molding method.

Method used

The superfine 3YSZ powder, pure zirconia powder and nano yttrium oxide powder were used to grind and disperse with composite binder and dispersant. After heat treatment and spheroidization treatment, a spherical zirconia grinding medium was prepared.

Benefits of technology

A simple process is realized to prepare sub-mm-level zirconia grinding media, which has good fluidity and high purity, high spherical shape, high density and high hardness, is suitable for mass production, and is suitable for grinding and dispersion of functional materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118878320A_ABST
    Figure CN118878320A_ABST
Patent Text Reader

Abstract

The invention provides a zirconium oxide grinding medium and a preparation method thereof, and belongs to the technical field of grinding media, and the preparation method comprises the following steps: S1, mixing superfine 3YSZ powder, pure zirconium oxide powder and nano yttrium oxide powder to obtain mixed powder, adding a composite binder, a dispersant, deionized water and n-butyl alcohol, and carrying out grinding dispersion to obtain uniformly dispersed and mixed slurry; s2, granulating the uniformly mixed slurry in the step S1 to obtain zirconium oxide granulated powder, and carrying out heat treatment on the zirconium oxide granulated powder to obtain degreased zirconium oxide granulated powder; and S3, sintering and spheroidizing the degreased zirconium oxide granulation powder to generate the spherical zirconium oxide grinding medium. The invention provides a zirconium oxide grinding medium and a preparation method thereof. The spherical zirconium oxide grinding medium at a submillimeter level is prepared by a simple process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of grinding media, and in particular to a zirconium oxide grinding medium and a preparation method thereof. Background Art

[0002] With the development of science and technology, powder materials are developing towards high purity, ultrafine and even nano-scale - the characteristics they possess can meet the needs of industrial technology development. For example, the positive and negative powder materials of new energy vehicle power batteries have high requirements for the fineness and purity of battery materials, and achieve uniform dispersion of battery slurry, thereby improving battery performance. There are two main types of powder material preparation processes: chemical and physical methods. The powder synthesized by chemical method has good fineness, but the preparation process produces waste gas and wastewater, which puts great pressure on environmental protection. At present, the ball milling method, which is a typical representative of physical method, is widely used in the powder industry - planetary ball milling, stirring mill, vibration mill, wet sand mill, etc. However, to achieve high purity and fineness of powder and uniform dispersion of slurry, advanced equipment and high-quality grinding media are required.

[0003] Zirconia ceramic balls have the characteristics of high density, high hardness, high wear resistance, high toughness and corrosion resistance. In production, they have high grinding efficiency, less wear and less impurities, showing more superior performance. They can be widely used as high-grade grinding media for fine powder processing and slurry dispersion equipment in ceramics, cement, chemical paints, coatings, pigments, medical, cosmetics and other industries.

[0004] At present, the main molding technologies used in the production of spherical zirconia grinding media are: plastic extrusion molding, isostatic pressing molding, rolling molding, etc. The plastic extrusion molding method is simple and has high production efficiency, but the performance of the molded products is low; the isostatic pressing method has excellent product performance, but for sub-millimeter spherical grinding media, the production efficiency is very low; the rolling molding method is conducive to the production of millimeter-level grinding media, but when preparing sub-millimeter-level spherical grinding media, the quality requirements of zirconia powder are high, and the process technology is difficult.

[0005] Therefore, it is necessary to provide a zirconium oxide grinding medium and a preparation method thereof to solve the problems existing in the above-mentioned prior art. Summary of the invention

[0006] In view of this, the present invention provides a zirconium oxide grinding medium and a preparation method thereof, so as to realize the preparation of sub-millimeter-level spherical zirconium oxide grinding media by a simple process.

[0007] To achieve the above object, the present invention provides a method for preparing a zirconium oxide grinding medium, comprising the following steps: S1, ultrafine 3YSZ powder, pure zirconium oxide powder and nano yttrium oxide powder are mixed to obtain a mixed powder, a composite binder, a dispersant, deionized water and n-butanol are added, and the mixture is ground and dispersed to obtain a dispersed and uniformly mixed slurry; S2, granulating the slurry mixed evenly in S1 to obtain zirconium oxide granulated powder, and heat-treating the zirconium oxide granulated powder to obtain defatted zirconium oxide granulated powder; S3, sintering and spheroidizing the defatted zirconium oxide granulated powder to generate spherical zirconium oxide grinding media.

[0008] The present invention uses ultrafine 3YSZ powder, pure zirconium oxide powder and nano yttrium oxide powder to mix three powders with different particle sizes, grinds and disperses with a composite binder and a dispersant to make the components evenly mixed, and prepares submillimeter-level zirconium oxide granulated powder by granulation. After subsequent heat treatment and degreasing, the spherical shape of the powder is maintained, and the powder has good fluidity. At the same time, the binder and the dispersant are removed, which is beneficial to the subsequent powder transportation, sintering and spheroidization. The whole preparation method has low process requirements and simple steps. The raw materials and the process are combined to prepare the submillimeter-level zirconium oxide grinding media.

[0009] Optionally, the composite binder in S1 is a mixture of polyvinyl alcohol and phenolic resin, and the mass ratio of polyvinyl alcohol to phenolic resin is 1:0.1~5; the mass ratio of mixed powder in S1:composite binder:dispersant:deionized water:n-butanol is 1:0.005~0.1:0.001~0.005:0.3~1:0.001~0.005.

[0010] Optionally, the ultrafine 3YSZ powder in S1 is an ultrafine 3 mol% yttrium-stabilized zirconia powder, the pure zirconia powder is a micro- or ultrafine ceramic powder with an average particle size not greater than 5.0 μm; the average particle size of the nano yttrium oxide powder is not greater than 0.1 μm; the average particle size of the mixed powder in S1 is 0.5~5.0 μm, and the particle size corresponding to 90% of the particle size distribution of the mixed powder is ≤8.0 μm; the viscosity of the uniformly mixed slurry in S1 is not greater than 2.0 Pa.s.

[0011] The average particle size of the mixed powder and the particle size corresponding to 90% of the particle size distribution of the mixed powder in the present invention can ensure that the solid content of the slurry in the later stage is higher within a certain viscosity range, which is conducive to the preparation of solid granulation powder, and is conducive to rapid sintering and spheroidization. The viscosity of the mixed slurry is limited in the present invention. If the viscosity exceeds the limit, the slurry transportation and atomization are difficult, which is not conducive to subsequent spray granulation.

[0012] Optionally, the granulation in S2 uses a spray granulator, and the working conditions of the spray granulator are as follows: the inlet temperature is 200-360°C, the outlet temperature is 70-140°C, the feed rate is 5-50kg / h, the carrier gas is air or inert gas, and the gas flow rate is 150-450Nm 3 / h; the spray granulator adopts an atomizing disk for atomization, and the rotation speed of the atomizing disk is 10000-23000rpm.

[0013] Optionally, the heat treatment in S2 includes heating up first and then cooling down, the heating rate is 5~50℃ / min, the heating end point is 500~1200℃, the holding time at the heating end point is 0.5~5h, and the cooling rate is 10~100℃ / min; the heat treatment conditions also include one or a combination of more than two of vacuum, inert atmosphere and reducing atmosphere.

[0014] In the present invention, the spherical shape of the powder is maintained by heat treatment, and the organic matter is removed cleanly, which is beneficial to the rapid sintering and spheroidization of S3.

[0015] Optionally, the vacuum degree of the vacuum is ≤13.3 Pa, the inert atmosphere is nitrogen, and the reducing atmosphere includes one or a mixture of two or more of hydrogen, methane, carbon monoxide, acetylene and nitrogen.

[0016] Optionally, the spheroidization treatment equipment in S3 is a plasma spheroidization furnace, and the spheroidization treatment conditions include that the gas forming the plasma is a mixture of argon and oxygen, the mixed gas and the generated spherical zirconia grinding media are separated by gas-solid separation and recycled by a purification device, and the temperature of the plasma flame is 1600~2700℃.

[0017] The invention utilizes the high temperature of plasma flame to carry out rapid sintering and spheroidization simultaneously, with short time and high efficiency, which is conducive to continuous industrial production.

[0018] Optionally, the dispersant in S1 is one or a combination of two or more of carboxylate, quaternary ammonium salt, oleyl amino oleate, polyvinyl pyrrolidone, sodium lauryl sulfate, and ammonium polymethacrylate.

[0019] Optionally, the spherical zirconia grinding media in S3 are classified to obtain spherical zirconia grinding media of different particle sizes, and the classification includes cyclone separation and screening.

[0020] The present invention can obtain spherical zirconium oxide grinding media with different particle sizes by combining granulation and classification, thereby meeting the demand for grinding media with different particle sizes.

[0021] In order to achieve the above object, the present invention also provides a zirconium oxide grinding medium prepared by the above method.

[0022] The particle size of the zirconium oxide grinding medium prepared by the present invention can reach sub-millimeter or even tens of microns, and the grinding medium has the characteristics of good spherical roundness, high density, high strength, high toughness, ultra-high wear resistance, long service life, high temperature resistance, non-conductivity, non-magnetism, and no pollution to materials, etc., which is helpful to realize nano-level grinding, crushing and dispersion of functional materials.

[0023] The above technical solution of the present invention includes at least the following beneficial effects: The present invention uses ultrafine 3YSZ powder, pure zirconium oxide powder and nano yttrium oxide powder to mix three powders with different particle sizes, grinds and disperses with a composite binder and a dispersant to make the components evenly mixed, and prepares submillimeter-level zirconium oxide granulated powder by granulation. After subsequent heat treatment and degreasing, the spherical shape of the powder is maintained, and the powder has good fluidity. At the same time, the binder and the dispersant are removed, which is beneficial to the subsequent powder transportation, sintering and spheroidization. The whole preparation method has low process requirements and simple steps. The raw materials and the process are combined to prepare the submillimeter-level zirconium oxide grinding media.

[0024] The preparation method used in the present invention can controllably prepare spherical zirconia grinding media with different particle sizes of sub-millimeter or even tens of microns, and the grinding media has high sphericity, high density, high hardness, high purity, high wear resistance, high toughness, and is suitable for mass production. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a SEM image of the nano yttrium oxide powder in Example 1 of the present invention; Figure 2 This is a SEM image of the defatted zirconium oxide granulated powder in Example 1 of the present invention; Figure 3 This is a SEM image of the zirconium oxide grinding medium prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0026] To make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the following will be combined with the appended drawings of the embodiments of the present invention. Figures 1 to 3 , the technical scheme of the embodiment of the present invention is clearly and completely described. Obviously, the described embodiment is a part of the embodiment of the present invention, not all of the embodiments. Based on the described embodiment of the present invention, all other embodiments obtained by ordinary technicians in this field belong to the scope of protection of the present invention.

[0027] Embodiment 1: 3YSZ (3% molar yttrium stabilized zirconia) zirconium oxide powder with an average particle size of 2.2 μm, pure zirconium oxide powder of 3.5 μm and nano yttrium oxide powder of 0.08 μm were mixed in a mass ratio of 50:46:4, and the average particle size of the mixed powder was 2.7 μm, and the particle size corresponding to 90% of the particle size distribution was 3 μm; the mixed powder was mixed with deionized water, composite binder, dispersant and n-butanol in a mass ratio of 1:0.33:0.03:0.002:0.0005, and put into a basket sand mill for grinding and dispersion for 24 hours to prepare zirconium oxide slurry. Among them, the composite binder is a mixture of polyvinyl alcohol and phenolic resin in a mass ratio of 1:1.25, and the dispersant is ammonium polymethacrylate.

[0028] The slurry was sprayed and granulated using a centrifugal spray dryer with a feed rate of 22 kg / h, inlet and outlet temperatures adjusted to 280 °C and 113 °C, respectively, atomizing disk speed of 19300 rpm, carrier gas of air, and gas flow rate of 200 Nm 3 / h (referring to the volume flow rate under standard conditions), a cyclone separator is used to extract particles with too small a particle size to obtain zirconium oxide granulated powder.

[0029] The obtained zirconium oxide granulated powder was placed in a heat treatment device, heated from room temperature to 1100°C under a hydrogen reducing atmosphere at a heating rate of 40°C / min, treated at 1100°C for 0.5h, cooled to room temperature at a cooling rate of 50°C / min, and degreased zirconium oxide granulated powder was obtained.

[0030] The defatted spherical zirconium oxide granulated powder is fed into the powder spheroidizing furnace by gas transportation at a feed rate of 8kg / h, and passes through the plasma flame zone. The center temperature of the plasma flame zone is controlled at 2200℃, and the spherical YSZ (yttrium stabilized zirconium oxide) grinding media is generated by rapid sintering and spheroidization. After the gas-solid separation device, the zirconium oxide grinding balls are quickly sintered and spheroidized and enter the collection tank. The separated gas is purified and reused.

[0031] The spherical YSZ (yttrium stabilized zirconia) grinding media is classified by a cyclone separator to obtain zirconium oxide grinding media.

[0032] Example 2 3YSZ (3% molar yttrium stabilized zirconia) zirconium oxide powder with an average particle size of 2.2 μm, pure zirconium oxide powder of 5 μm and nano yttrium oxide powder of 0.1 μm were mixed in a mass ratio of 50:45:5, and the average particle size of the mixed powder was 3.35 μm, and the particle size corresponding to 90% of the particle size distribution was 3.6 μm; the mixed powder was mixed with deionized water, composite binder, dispersant and n-butanol in a mass ratio of 1:1:0.1:0.005:0.0003, and put into a basket sand mill for grinding and dispersion for 20 hours to prepare zirconium oxide slurry. Among them, the composite binder is a mixture of polyvinyl alcohol and phenolic resin in a mass ratio of 1:5, and the dispersant is polyvinyl pyrrolidone.

[0033] The slurry was sprayed and granulated using a centrifugal spray dryer with a feed rate of 5 kg / h, inlet and outlet temperatures adjusted to 200 °C and 70 °C, atomizing disk speed of 10,000 rpm, inert gas as carrier gas, and a gas flow rate of 150 Nm 3 / h (referring to the volume flow rate under standard conditions), a cyclone separator is used to extract particles with too small a particle size to obtain zirconium oxide granulated powder.

[0034] The obtained zirconium oxide granulated powder was placed in a heat treatment equipment, heated from room temperature to 1200°C at a vacuum degree of 13.3 Pa, with a heating rate of 50°C / min, treated at 1200°C for 5 hours, cooled to room temperature at a cooling rate of 100°C / min, and degreased zirconium oxide granulated powder was obtained.

[0035] The defatted spherical zirconium oxide granulated powder is fed into the powder spheroidizing furnace by gas transportation at a feed rate of 10kg / h, and passes through the plasma flame zone. The center temperature of the plasma flame zone is controlled at 2700℃, and the spherical YSZ (yttrium stabilized zirconium oxide) grinding media is generated by rapid sintering and spheroidization. After the gas-solid separation device, the zirconium oxide grinding balls are quickly sintered and spheroidized and enter the collection tank. The separated gas is purified and reused.

[0036] The spherical YSZ (yttrium stabilized zirconia) grinding media is classified by a cyclone separator to obtain zirconium oxide grinding media.

[0037] Example 3 3YSZ (3% molar yttrium stabilized zirconia) zirconium oxide powder with an average particle size of 2.2 μm, pure zirconium oxide powder with a particle size of 0.8 μm and nano yttrium oxide powder with a particle size of 0.05 μm were mixed in a mass ratio of 50:40:10, and the average particle size of the mixed powder was 1.42 μm, and the particle size corresponding to 90% of the particle size distribution was 1.5 μm; the mixed powder was mixed with deionized water, composite binder, dispersant and n-butanol in a mass ratio of 1:0.6:0.005:0.001:0.0001, and put into a basket sand mill for grinding and dispersion for 28 hours to prepare zirconium oxide slurry. Among them, the composite binder is a mixture of polyvinyl alcohol and phenolic resin in a mass ratio of 1:0.1, and the dispersant is ammonium polymethacrylate.

[0038] The slurry was sprayed and granulated using a centrifugal spray dryer with a feed rate of 50 kg / h, inlet and outlet temperatures adjusted to 360 °C and 140 °C, respectively, atomizing disk speed of 23000 rpm, carrier gas of air, and gas flow rate of 450 Nm 3 / h (referring to the volume flow rate under standard conditions), a cyclone separator is used to extract particles with too small a particle size to obtain zirconium oxide granulated powder.

[0039] The obtained zirconium oxide granulated powder was placed in a heat treatment device, heated from room temperature to 500°C under a nitrogen atmosphere at a heating rate of 5°C / min, treated at 500°C for 2.5h, cooled to room temperature at a cooling rate of 40°C / min, and degreased zirconium oxide granulated powder was obtained.

[0040] The defatted spherical zirconium oxide granulated powder is fed into the powder spheroidizing furnace by gas transportation at a feed rate of 6kg / h, and passes through the plasma flame zone. The center temperature of the plasma flame zone is controlled at 1600℃, and the spherical YSZ (yttrium stabilized zirconium oxide) grinding media is generated by rapid sintering and spheroidization. After the gas-solid separation device, the zirconium oxide grinding balls are quickly sintered and spheroidized and enter the collection tank. The separated gas is purified and reused.

[0041] The spherical YSZ (yttrium stabilized zirconia) grinding media is classified by a cyclone separator to obtain zirconium oxide grinding media.

[0042] Example 4 The only difference from Example 1 is that the dispersant is a mixture of sodium lauryl sulfate and oleyl amino oleate.

[0043] Comparative Example 1 Compared with Example 1, the only difference is that no thermal degreasing is used.

[0044] Comparative Example 2 Compared with Example 1, the only difference is that the binder used is polyvinyl alcohol alone.

[0045] Comparative Example 3 Compared with Example 1, the only difference is that the binder used is a single phenolic resin.

[0046] The performance of the zirconium oxide grinding media prepared in Examples 1 to 4 and Comparative Examples 1 to 3 was tested, and the results are shown in Table 1.

[0047] Table 1 Performance of the zirconium oxide grinding media prepared in Examples 1 to 4 and Comparative Examples 1 to 3

[0048] According to the data in Table 1, the zirconia grinding media prepared in Examples 1 to 4 of the present invention have stronger performance than the zirconia grinding media prepared in Comparative Examples 1 to 3, and have advantages in sphericity, density, strength, hardness and elastic modulus over the zirconia grinding media prepared in Comparative Examples 1 to 3.

[0049] The nano yttrium oxide powder, the defatted zirconium oxide granulated powder and the prepared zirconium oxide grinding medium in Example 1 were respectively subjected to electron microscope scanning to obtain Figure 1 , Figure 2 and Figure 3 .

[0050] Figure 2 It shows that the degreased zirconium oxide granulated powder of the present invention maintains a good spherical shape, and the organic matter attached to the surface is completely removed, which is conducive to subsequent rapid sintering and spheroidization. Figure 3 It shows that the obtained zirconium oxide grinding media is spherical and uniform, and the particle size reaches sub-millimeter level.

[0051] The above are preferred embodiments of the present invention. It should be pointed out that, for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as within the scope of protection of the present invention.

Claims

1. A method for preparing a zirconium oxide grinding medium, characterized in that: The following steps are involved: S1, ultrafine 3YSZ powder, pure zirconium oxide powder and nano yttrium oxide powder are mixed to obtain a mixed powder, a composite binder, a dispersant, deionized water and n-butanol are added, and the mixture is ground and dispersed to obtain a dispersed and uniformly mixed slurry; S2, granulating the slurry mixed evenly in S1 to obtain zirconium oxide granulated powder, and heat-treating the zirconium oxide granulated powder to obtain defatted zirconium oxide granulated powder; S3, sintering and spheroidizing the defatted zirconium oxide granulated powder to generate spherical zirconium oxide grinding media.

2. The method for preparing the zirconium oxide grinding medium according to claim 1, characterized in that: The composite binder in S1 is obtained by mixing polyvinyl alcohol and phenolic resin, and the mass ratio of polyvinyl alcohol to phenolic resin is 1:0.1-5; the mass ratio of mixed powder in S1:composite binder:dispersant:deionized water:n-butanol is 1:0.005-0.1:0.001-0.005:0.3-1:0.001-0.

005.

3. The method for preparing the zirconium oxide grinding medium according to claim 1, characterized in that: The ultrafine 3YSZ powder in S1 is an ultrafine 3% molar yttrium-stabilized zirconia powder, the pure zirconia powder is a fine or ultrafine ceramic powder with an average particle size not greater than 5.0 μm; the average particle size of the nano yttrium oxide powder is not greater than 0.1 μm; the average particle size of the mixed powder in S1 is 0.5~5.0 μm, and the particle size corresponding to 90% of the particle size distribution of the mixed powder is ≤8.0 μm; the viscosity of the uniformly mixed slurry in S1 is not greater than 2.0 Pa.s.

4. The method for preparing the zirconium oxide grinding medium according to claim 1, characterized in that: The granulation in S2 uses a spray granulator, and the working conditions of the spray granulator are as follows: the inlet temperature is 200-360°C, the outlet temperature is 70-140°C, the feed rate is 5-50kg / h, the carrier gas is air or inert gas, and the gas flow rate is 150-450Nm 3 / h; the spray granulator adopts an atomizing disk for atomization, and the rotation speed of the atomizing disk is 10000-23000rpm.

5. The method for preparing the zirconium oxide grinding medium according to claim 1, characterized in that: The heat treatment in S2 includes heating up first and then cooling down, the heating rate is 5-50°C / min, the heating end point is 500-1200°C, the holding time at the heating end point is 0.5-5h, and the cooling rate is 10-100°C / min; the heat treatment conditions also include one or a combination of more than two of vacuum, inert atmosphere and reducing atmosphere.

6. The method for preparing the zirconium oxide grinding medium according to claim 5, characterized in that: The vacuum degree of the vacuum is ≤13.3 Pa, the inert atmosphere is nitrogen, and the reducing atmosphere includes one or a mixture of two or more of hydrogen, methane, carbon monoxide, acetylene and nitrogen.

7. The method for preparing the zirconium oxide grinding medium according to claim 1, characterized in that: The spheroidizing treatment equipment in S3 is a plasma spheroidizing furnace. The spheroidizing treatment conditions include that the gas forming the plasma is a mixture of argon and oxygen. The mixture is separated from the generated spherical zirconia grinding media by gas-solid separation and recycled by a purification device. The temperature of the plasma flame is 1600~2700℃.

8. The method for preparing the zirconium oxide grinding medium according to claim 1, characterized in that: The dispersant in S1 is one or a combination of two or more of carboxylate, quaternary ammonium salt, polyvinyl pyrrolidone, sodium lauryl sulfate, oleyl amino oleate, and ammonium polymethacrylate.

9. The method for preparing the zirconium oxide grinding medium according to claim 1, characterized in that: The spherical zirconia grinding media in S3 are classified to obtain spherical zirconia grinding media of different particle sizes, and the classification includes cyclone separation and screening.

10. A zirconium oxide grinding medium prepared by the method for preparing a zirconium oxide grinding medium according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Preparation method of yttrium oxide-stabilized zirconia pelletized powder

    CN104129989A