Modified waterborne alkyd resin and preparation method thereof
Through the process of alcoholylation, esterification and modification treatment, the water resistance and drying speed of the aqueous alkyd resin are improved, the hardness of the paint film is enhanced, and the problem of insufficient performance of the existing aqueous alkyd resin is solved.
Patent Information
- Application Number
- CN202411114049.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The water resistance, drying speed and paint film hardness of existing aqueous alkyd resins still need to be improved.
By alcoholizing the vegetable oil with polyol, then esterifying with benzoic acid, and adding epoxy resin and antioxidant to the reflux reaction of the acid anhydride for modification, a modified aqueous alkyd resin was formed.
The water resistance and drying speed of the aqueous alkyd resin are significantly improved, while the hardness of the paint film is enhanced.
Smart Images

Figure CN118878802A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials, and in particular to a modified waterborne alkyd resin and a preparation method thereof. Background Art
[0002] Alkyd resin is a very important chemical product, which is widely used in coatings, inks and other fields. Water-based alkyd resin is the development direction of alkyd resin, which also meets environmental protection requirements. However, compared with solvent-based alkyd resin, water-based alkyd resin still has the following technical defects: easy hydrolysis, poor water resistance and insufficient stability.
[0003] Based on this, existing patent technologies have proposed a variety of different waterborne alkyd resin modification methods. For example, Chinese patent CN111040141 A discloses a waterborne alkyd resin and its application, which utilizes the steric hindrance effect of the ethyl group on trimethylolpropane to protect the ester bond of the polyester, so that the prepared waterborne alkyd resin has hydrolysis resistance, antioxidant stability, alkali resistance, and thermal stability, and the combination of ethylene glycol and pentaerythritol can adjust the functionality, stabilize the polymerization, and avoid gelation.
[0004] Chinese patent CN111995715A discloses a preparation method of a step-by-step modified waterborne alkyd resin and a waterborne alkyd resin, which includes the preparation of an acrylic prepolymer, the preparation of an acrylic modified waterborne alkyd resin, and the preparation of a styrene modified waterborne alkyd resin. This patent uses a step-by-step modification process to reduce the loss of double bonds in the molecule. The prepared waterborne alkyd resin combines the advantages of acrylic acid and styrene on the basis of traditional alkyd resin, and has the characteristics of environmental protection, good water solubility, high hardness, fast drying speed, etc.
[0005] According to the existing research results, the water resistance of the currently prepared water-based alkyd resin still needs to be further improved. Summary of the invention
[0006] In view of this, the present invention provides a modified waterborne alkyd resin and a preparation method thereof. The present invention firstly performs alcoholysis on vegetable oil and polyol to obtain alcoholysis product; then performs esterification on the alcoholysis product and benzoic acid to obtain alkyd resin; then performs reflux reaction on the alkyd resin and composite acid anhydride to obtain waterborne alkyd resin; finally, the waterborne alkyd resin is modified by epoxy resin and antioxidant under the action of initiator and cosolvent to obtain modified waterborne alkyd resin. The present invention is implemented by the following technical scheme:
[0007] A modified waterborne alkyd resin comprises the following raw materials in parts by weight:
[0008] Epoxy resin 2-5 parts;
[0009] 5-10 parts of benzoic acid;
[0010] 10-20 parts of polyol;
[0011] 30-50 parts of vegetable oil;
[0012] 3-7 parts of acid anhydride;
[0013] Catalyst 0.1-0.5 parts;
[0014] Initiator 0.1-0.2 parts;
[0015] 10-20 parts of cosolvent;
[0016] 0.5-3 parts of antioxidant;
[0017] The acid anhydride is a mixture of trimellitic anhydride and phthalic anhydride in a mass ratio of 1:2-3;
[0018] The cosolvent is a mixture of propylene glycol methyl ether acetate and arachidyl alcohol in a mass ratio of 3:1.
[0019] Preferably, the polyol is one or more of ethylene glycol, propylene glycol and pentaerythritol.
[0020] Preferably, the vegetable oil is one or more of soybean oil, tung oil and linseed oil.
[0021] Preferably, the catalyst is lithium hydroxide.
[0022] Preferably, the initiator is azobisisobutyronitrile.
[0023] Preferably, the antioxidant is one of triphenyl phosphite or triphenyl phosphate.
[0024] The present invention also provides a method for preparing the modified waterborne alkyd resin, comprising the following steps:
[0025] (1) Alcoholysis: weigh the raw materials according to the proportion, then add the vegetable oil into the reactor, start stirring, add the polyol when the temperature reaches 70-90°C, add the catalyst when the temperature continues to rise to 120-140°C, heat to 240-250°C and keep the temperature for reaction for 1-2 hours, and obtain the alcoholysis product after the reaction is completed;
[0026] (2) esterification: adding weighed benzoic acid to the alcoholysis product, heating and heating to carry out reflux esterification reaction, and obtaining an alkyd resin after the reaction is completed;
[0027] (3) water-based: adding the weighed acid anhydride to the alkyd resin and continuing to heat it to reflux reaction, and obtaining a water-based material after the reaction is completed;
[0028] (4) Modification treatment: adding an antioxidant, a cosolvent and an epoxy resin to the aqueous material and stirring the mixture to react, thereby obtaining a modified aqueous alkyd resin.
[0029] Preferably, the esterification reaction time in step (2) is 2 to 3 hours.
[0030] Preferably, the reflux reaction time in step (3) is 1 to 2 hours.
[0031] Preferably, the stirring temperature in step (4) is 45-55°C.
[0032] Compared with the prior art, the present invention has the following beneficial effects:
[0033] The invention provides a modified water-based alkyd resin and a preparation method thereof. The invention uses a composite acid anhydride to react with an alkyd resin to obtain a water-based alkyd resin, and then adds an epoxy resin and a composite cosolvent for modification, thereby significantly improving the water resistance of the water-based alkyd resin, and also improving the drying speed and paint film hardness of the water-based alkyd resin. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 The present invention is a process flow chart for preparing the modified waterborne alkyd resin. DETAILED DESCRIPTION
[0035] The present invention is further described below in conjunction with the examples. The epoxy resin used in the following examples and comparative examples of the present invention is epoxy resin E44, which was purchased from Shaanxi Lanxin Chemical Co., Ltd.
[0036] Example 1
[0037] A modified waterborne alkyd resin is prepared from the following raw materials in parts by weight:
[0038] Epoxy resin 3 parts;
[0039] 8 parts of benzoic acid;
[0040] Polyol (propylene glycol) 15 parts;
[0041] 35 parts of vegetable oil (tung oil);
[0042] 5 parts of acid anhydride;
[0043] Catalyst (lithium hydroxide) 0.5 part;
[0044] Initiator (azobisisobutyronitrile) 0.2 parts;
[0045] 15 parts of cosolvent;
[0046] Antioxidant (triphenyl phosphite) 2 parts;
[0047] The acid anhydride is a mixture of trimellitic anhydride and phthalic anhydride in a mass ratio of 1:2;
[0048] The cosolvent is a mixture of propylene glycol methyl ether acetate and arachidyl alcohol in a mass ratio of 3:1.
[0049] The preparation method of the modified waterborne alkyd resin of the present invention comprises the following steps:
[0050] (1) Alcoholysis: weigh the raw materials according to the proportion, then add the vegetable oil into the reactor, start stirring, add the polyol (propylene glycol) when the temperature reaches 80°C, add the catalyst when the temperature continues to rise to 130°C, heat to 240°C and keep the temperature for reaction for 1.5 hours, and obtain the alcoholysis product after the reaction is completed;
[0051] (2) Esterification: adding weighed benzoic acid to the alcoholysis product, heating and reflux esterification for 2.5 hours, and obtaining an alkyd resin after the reaction is completed;
[0052] (3) water-based: adding the weighed acid anhydride to the alkyd resin and continuing to heat to reflux for 1.5 hours, and obtaining a water-based material after the reaction is completed;
[0053] (4) Modification treatment: After adding an antioxidant, a cosolvent and an epoxy resin to the aqueous material, stirring and reacting the mixture at a temperature of 50° C., a modified aqueous alkyd resin is obtained.
[0054] Example 2
[0055] A modified waterborne alkyd resin is prepared from the following raw materials in parts by weight:
[0056] Epoxy resin 3 parts;
[0057] 8 parts of benzoic acid;
[0058] Polyol (ethylene glycol) 15 parts;
[0059] 35 parts of vegetable oil (linseed oil);
[0060] 5 parts of acid anhydride;
[0061] Catalyst (lithium hydroxide) 0.5 part;
[0062] Initiator (azobisisobutyronitrile) 0.2 parts;
[0063] 15 parts of cosolvent;
[0064] Antioxidant (triphenyl phosphate) 2 parts;
[0065] The acid anhydride is a mixture of trimellitic anhydride and phthalic anhydride in a mass ratio of 1:3;
[0066] The cosolvent is a mixture of propylene glycol methyl ether acetate and arachidyl alcohol in a mass ratio of 3:1.
[0067] The steps and parameter settings in the preparation method of the modified waterborne alkyd resin in this embodiment are the same as those in Example 1.
[0068] Example 3
[0069] A modified waterborne alkyd resin is prepared from the following raw materials in parts by weight:
[0070] Epoxy resin 3 parts;
[0071] 8 parts of benzoic acid;
[0072] Polyol (pentaerythritol) 15 parts;
[0073] Vegetable oil (soybean oil) 35 parts;
[0074] 5 parts of acid anhydride;
[0075] Catalyst (lithium hydroxide) 0.5 parts;
[0076] Initiator (azobisisobutyronitrile) 0.2 parts;
[0077] 15 parts of cosolvent;
[0078] 2 parts of antioxidant (triphenyl phosphate);
[0079] The acid anhydride is a mixture of trimellitic anhydride and phthalic anhydride in a mass ratio of 1:2;
[0080] The cosolvent is a mixture of propylene glycol methyl ether acetate and arachidyl alcohol in a mass ratio of 3:1.
[0081] The steps and parameter settings in the preparation method of the modified waterborne alkyd resin in this embodiment are the same as those in Example 1.
[0082] The steps and parameter settings in the preparation method of the modified waterborne alkyd resin in this embodiment are the same as those in Example 1.
[0083] The raw material systems of the modified waterborne alkyd resins in Examples 1 and 2-3 are shown in Tables 1 and 2.
[0084] Table 1
[0085]
[0086] The modified waterborne alkyd resin prepared in Examples 1-3 was tested for performance, wherein the test method for the paint film hardness was based on GB / T1730-2007B; the test methods for the surface drying time and the actual drying time were based on GB / T1728-1989, as shown in Table 2. The water resistance test method was based on GB / T1733-1993;
[0087] Table 2
[0088] Film hardness Dry time Working time Water resistance Example 1 0.90 10min 25min 14d No change Example 2 0.87 15min 32min 14d No change Example 3 0.81 18min 40min 14d No change
[0089] Embodiment 4-5
[0090] A modified waterborne alkyd resin, having the same raw material types as those in Example 1, except that the weight portions of the raw materials are adjusted, as shown in Table 3.
[0091] Table 3
[0092]
[0093]
[0094] The performance of the modified waterborne alkyd resins prepared in Example 4 and Example 5 was tested, as shown in Table 4.
[0095] Table 4
[0096] Film hardness Dry time Working time Water resistance Example 1 0.90 10min 25min 14d No change Example 4 0.88 12min 28min 14d No change Example 5 0.89 11min 27min 14d No change
[0097] Example 6
[0098] A modified waterborne alkyd resin, having the same raw materials as those in Example 1, except that the preparation process parameters are adjusted. The specific preparation process is as follows:
[0099] (1) Alcoholysis: weigh the raw materials according to the proportion, then add the vegetable oil into the reactor, start stirring, add the polyol (propylene glycol) when the temperature reaches 70°C, add the catalyst when the temperature continues to rise to 120°C, heat to 250°C and keep the temperature for 2 hours, and obtain the alcoholysis product after the reaction is completed;
[0100] (2) Esterification: adding weighed benzoic acid to the alcoholysis product, heating and reflux esterification for 3 hours, and obtaining an alkyd resin after the reaction is completed;
[0101] (3) water-based: adding the weighed acid anhydride to the alkyd resin and continuing to heat it to reflux for 2 hours, and obtaining a water-based material after the reaction is completed;
[0102] (4) Modification treatment: After adding an antioxidant, a cosolvent and an epoxy resin to the aqueous material, stirring and reacting the mixture at a temperature of 55° C., a modified aqueous alkyd resin is obtained.
[0103] The performance test of the modified waterborne alkyd resin prepared in Example 6 was basically the same as that in Example 1.
[0104] Comparative Example 1
[0105] A method for preparing a modified waterborne alkyd resin is described in Example 1, except that the acid anhydride used is trimellitic anhydride, the cosolvent used is propylene glycol methyl ether acetate, and no epoxy resin is added. The details are as follows:
[0106] A modified waterborne alkyd resin is prepared from the following raw materials in parts by weight:
[0107] 8 parts of benzoic acid;
[0108] Polyol (propylene glycol) 15 parts;
[0109] 35 parts of vegetable oil (tung oil);
[0110] 5 parts of acid anhydride;
[0111] Catalyst (lithium hydroxide) 0.5 parts;
[0112] Initiator (azobisisobutyronitrile) 0.2 parts;
[0113] 15 parts of cosolvent;
[0114] Antioxidant (triphenyl phosphite) 2 parts;
[0115] wherein the acid anhydride is trimellitic anhydride;
[0116] The cosolvent is propylene glycol methyl ether acetate.
[0117] The preparation method of the modified waterborne alkyd resin of the present invention comprises the following steps:
[0118] (1) Alcoholysis: weigh the raw materials according to the proportion, then add the vegetable oil into the reactor, start stirring, add the polyol (propylene glycol) when the temperature reaches 80°C, add the catalyst when the temperature continues to rise to 130°C, heat to 240°C and keep the temperature for reaction for 1.5 hours, and obtain the alcoholysis product after the reaction is completed;
[0119] (2) Esterification: adding weighed benzoic acid to the alcoholysis product, heating and reflux esterification for 2.5 hours, and obtaining an alkyd resin after the reaction is completed;
[0120] (3) water-based: adding the weighed acid anhydride to the alkyd resin and continuing to heat to reflux for 1.5 hours, and obtaining a water-based material after the reaction is completed;
[0121] (4) Modification treatment: After adding an antioxidant and a cosolvent to the aqueous material, stirring and reacting the mixture at a temperature of 50° C., a modified aqueous alkyd resin is obtained.
[0122] Comparative Example 2
[0123] A water-based alkyd resin is prepared from the following raw materials in parts by weight:
[0124] 8 parts of benzoic acid;
[0125] Polyol (propylene glycol) 15 parts;
[0126] 35 parts of vegetable oil (tung oil);
[0127] 5 parts of acid anhydride;
[0128] Catalyst (lithium hydroxide) 0.5 parts;
[0129] The acid anhydride is a mixture of trimellitic anhydride and phthalic anhydride in a mass ratio of 1:2;
[0130] The preparation method of the water-based alkyd resin in the present embodiment comprises the following steps:
[0131] (1) Alcoholysis: weigh the raw materials according to the proportion, then add the vegetable oil into the reactor, start stirring, add the polyol (propylene glycol) when the temperature reaches 80°C, add the catalyst when the temperature continues to rise to 130°C, heat to 240°C and keep the temperature for reaction for 1.5 hours, and obtain the alcoholysis product after the reaction is completed;
[0132] (2) Esterification: adding weighed benzoic acid to the alcoholysis product, heating and reflux esterification for 2.5 hours, and obtaining an alkyd resin after the reaction is completed;
[0133] (3) water-based: adding the weighed acid anhydride to the alkyd resin and continuing to heat it to reflux for 1.5 hours, and obtaining a water-based alkyd resin after the reaction is completed;
[0134] The modified waterborne alkyd resin prepared in Comparative Document 1 and the waterborne alkyd resin prepared in Comparative Document 2 were subjected to performance tests, as shown in Table 5.
[0135] Table 5
[0136] Film hardness Dry time Working time Water resistance Example 1 0.90 10min 25min 14d No change Comparative Example 1 0.52 55min 72min Whitening and blistering after 5 days Comparative Example 2 0.40 65min 85min Whitening and blistering after 3d
[0137] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A modified waterborne alkyd resin, characterized in that: The invention comprises the following raw materials in parts by weight: Epoxy resin 2-5 parts; 5-10 parts of benzoic acid; 10-20 parts of polyol; 30-50 parts of vegetable oil; 3-7 parts of acid anhydride; Catalyst 0.1-0.5 parts; Initiator 0.1-0.2 parts; 10-20 parts of cosolvent; 0.5-3 parts of antioxidant; The acid anhydride is a mixture of trimellitic anhydride and phthalic anhydride in a mass ratio of 1:2-3; The cosolvent is a mixture of propylene glycol methyl ether acetate and arachidyl alcohol in a mass ratio of 3:
1.
2. A modified waterborne alkyd resin according to claim 1, characterized in that: The polyol is one or more of ethylene glycol, propylene glycol and pentaerythritol.
3. A modified waterborne alkyd resin according to claim 1, characterized in that: The vegetable oil is one or more of soybean oil, tung oil and linseed oil.
4. A modified waterborne alkyd resin according to claim 1, characterized in that: The catalyst is lithium hydroxide.
5. A modified waterborne alkyd resin according to claim 1, characterized in that: The initiator is azobisisobutyronitrile.
6. A modified waterborne alkyd resin according to claim 1, characterized in that: The antioxidant is one of triphenyl phosphite and triphenyl phosphate.
7. The method for preparing a modified waterborne alkyd resin according to any one of claims 1 to 6, characterized in that: The following steps are involved: (1) Alcoholysis: weigh the raw materials according to the proportion, then add the vegetable oil into the reactor, start stirring, add the polyol when the temperature reaches 70-90°C, add the catalyst when the temperature continues to rise to 120-140°C, heat to 240-250°C and keep the temperature for reaction for 1-2 hours, and obtain the alcoholysis product after the reaction is completed; (2) esterification: adding weighed benzoic acid to the alcoholysis product, heating and heating to carry out reflux esterification reaction, and obtaining an alkyd resin after the reaction is completed; (3) water-based: adding the weighed acid anhydride to the alkyd resin and continuing to heat it to reflux reaction, and obtaining a water-based material after the reaction is completed; (4) Modification treatment: adding an antioxidant, a cosolvent and an epoxy resin to the aqueous material and stirring the mixture to react, thereby obtaining a modified aqueous alkyd resin.
8. The preparation method according to claim 7, characterized in that: The esterification reaction time in step (2) is 2 to 3 hours.
9. The preparation method according to claim 7, characterized in that: The reflux reaction time in step (3) is 1 to 2 hours.
10. The preparation method according to claim 7, characterized in that: The stirring temperature in step (4) is 45-55°C.
Citation Information
Patent Citations
Epoxy modified prickly ash seed oil water-based alkyd amino-baking varnish and preparation method thereof
CN107216782A
Water-based alkyd resin and application thereof
CN111040141A