Polyformaldehyde composite material and preparation method thereof

By adding polytetrafluoroethylene micropowder, glass fiber and polyethylene glycol to the polyformaldehyde composite material, the proportion of components is controlled, and the problems of high friction coefficient and large wear are solved, and low friction is achieved The effect of coefficient, low wear amount and high wear resistance is suitable for the manufacturing of high-demand transmission parts.

CN118879017APending Publication Date: 2024-11-01CHINA ENERGY GRP NINGXIA COAL IND CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411194159.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

During use, existing polyformaldehyde composite materials have high friction coefficient, large wear amount, insufficient wear resistance, and low cost performance, which cannot meet the requirements for long-term use under high load and high sliding speed.

Method used

By using the preparation method of polyformaldehyde composite, by adding polytetrafluoroethylene micropowder, glass fiber, polyethylene glycol and antioxidants to polyformaldehyde, the proportion of each component is controlled, and the friction performance and wear resistance are synergistically improved, and the friction performance and wear resistance are reduced. Coefficient of friction and wear.

Benefits of technology

It significantly reduces the friction coefficient and wear amount of polyformaldehyde composite materials, improves its wear resistance and mechanical properties, extends the service life of the material, and improves energy use efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005015881700000071
    Figure BDA0005015881700000071
  • Figure BDA0005015881700000081
    Figure BDA0005015881700000081
  • Figure BDA0005015881700000091
    Figure BDA0005015881700000091
Patent Text Reader

Abstract

The invention provides a polyformaldehyde composite material, which is prepared from the following ingredients in parts by weight: 70 to 95 parts of polyformaldehyde, 1 to 10 parts of polytetrafluoroethylene micro powder, 1 to 10 parts of glass fibers, 1 to 7 parts of polyethylene glycol, 0.5 to 1 part of antioxidants and 0.5 to 2 parts of lubricating agents. Wherein the weight-average molecular weight of the polyethylene glycol is 5000 to 6000. The polyformaldehyde composite material prepared by using the preparation method provided by the invention has the advantages that the friction coefficient is reduced, the abrasion loss is reduced, the abrasion resistance is obviously improved, the durability of the material in use is facilitated, the use efficiency of energy is further improved, and the energy conservation is facilitated. In addition, based on the excellent performance of the polyformaldehyde composite material, the polyformaldehyde composite material can also be applied to special fields with high requirements on materials, such as precise transmission part manufacturing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of plastics, and in particular to a polyoxymethylene composite material and a preparation method thereof. Background Art

[0002] At present, the commonly used wear-resistant materials mainly include various metals and alloy materials, engineering ceramic materials, engineering plastics and composite materials with added fillers. Among them, engineering plastics with polymer as wear-resistant materials have the following advantages: low friction coefficient, good wear resistance, self-lubricating performance, and the wear resistance of the material can be greatly improved by further modification with modifiers. It can work under oil-free or low-oil conditions, and its corrosion resistance and processability will also be better.

[0003] Among commonly used engineering plastics, polyoxymethylene (POM) has mechanical properties that are superior to other plastics. It is known as "steel" and "super steel" and has a wide range of applications. As a well-known engineering plastic, POM has extremely high strength and rigidity, excellent self-lubricating properties, corrosion resistance and dimensional stability. It can replace metals in many occasions and is widely used in electronics, machinery, instrumentation, daily light industry, automobiles, building materials, agriculture and other fields. However, if we only rely on the inherent wear resistance of pure POM resin, especially under high loads and high sliding speeds, it cannot meet the requirements of long-term use of sliding parts. In particular, the friction coefficient between POM resin material and steel ring increases rapidly, resulting in an increase in wear.

[0004] POM can be classified according to whether there are ethoxy groups in the molecular chain, including homopolymer POM and copolymer POM. Because the ethoxy groups in the molecular chain can effectively terminate the chain decomposition, copolymer POM has good thermal stability, chemical stability, easy processing and other advantages. Currently, copolymer POM accounts for a higher proportion in the market, with a market share of more than 80%.

[0005] In summary, the exploration of the friction properties of POM and its composites is of great significance to production and life, and also helps to save energy and improve energy efficiency. Obtaining POM composites with lower friction coefficient and wear rate is a hot topic in recent research.

[0006] Although there have been studies on POM and its composite materials, the problem of improving the friction performance of POM and its composite materials has not been effectively solved. Therefore, it has become an urgent need in the current research field to develop a special POM material that meets practical requirements with low friction coefficient, low wear, high wear resistance and high cost performance. Summary of the invention

[0007] The main purpose of the present invention is to provide a polyoxymethylene composite material and a preparation method thereof, so as to solve the problems of high friction coefficient, large wear, insufficient wear resistance and low cost performance of the polyoxymethylene composite material in the prior art during use.

[0008] In order to solve the above problems, the present invention provides a polyoxymethylene composite material, which comprises the following components in parts by weight: 70 to 95 parts of polyoxymethylene, 1 to 10 parts of polytetrafluoroethylene powder, 1 to 10 parts of glass fiber, 1 to 7 parts of polyethylene glycol, 0.5 to 1 part of antioxidant, and 0.5 to 2 parts of lubricant; wherein the weight average molecular weight of the polyethylene glycol is 5000 to 6000.

[0009] Further, the polyoxymethylene composite material comprises the following components in parts by weight: 85-95 parts of polyoxymethylene, 1-5 parts of polytetrafluoroethylene powder, 1-5 parts of glass fiber, 1-3 parts of polyethylene glycol, 0.5-1 part of antioxidant, and 1-2 parts of lubricant; preferably, the polyoxymethylene composite material comprises the following components in parts by weight: 91 parts of polyoxymethylene, 3 parts of polytetrafluoroethylene powder, 1 part of glass fiber, 3 parts of polyethylene glycol, 0.5 part of antioxidant, and 1.5 parts of lubricant, and the weight average molecular weight of polyethylene glycol is 6000; or The polyoxymethylene composite material comprises the following components, by weight: 91 parts of polyoxymethylene, 4 parts of polytetrafluoroethylene powder, 1 part of glass fiber, 3 parts of polyethylene glycol, 0.5 parts of antioxidant, 0.5 parts of lubricant, and the weight average molecular weight of polyethylene glycol is 6000; or, the polyoxymethylene composite material comprises the following components, by weight: 89.5 parts of polyoxymethylene, 4 parts of polytetrafluoroethylene powder, 2 parts of glass fiber, 2 parts of polyethylene glycol, 0.5 parts of antioxidant, 2 parts of lubricant, and the weight average molecular weight of polyethylene glycol is 5000.

[0010] Furthermore, the polyoxymethylene is copolymer polyoxymethylene; preferably, the melt flow rate of the copolymer polyoxymethylene at 190° C. is 9 to 27 g / 10 min; further preferably, the brand of the copolymer polyoxymethylene is at least one of MC90, MC270, and MC140.

[0011] Furthermore, the particle size of the polytetrafluoroethylene powder is 5 to 10 μm; preferably, the melt flow rate of the polytetrafluoroethylene powder at 350° C. is 5 to 6 g / 10 min.

[0012] Furthermore, the fiber length of the glass fiber is 5 to 20 mm, and the diameter is 9 to 13 μm; preferably, the density of the glass fiber is 2.6 to 2.7 g / cm 3 .

[0013] Furthermore, the antioxidant is a hindered phenol antioxidant; preferably, the hindered phenol antioxidant is antioxidant 1010; preferably, the lubricant is silicone oil and / or mineral oil.

[0014] According to another aspect of the present invention, a method for preparing a polyoxymethylene composite material is also provided, the method comprising the following steps: S1: mixing and drying polyoxymethylene, polytetrafluoroethylene powder, glass fiber, and polyethylene glycol to obtain a dried mixture;

[0015] S2: Melting and mixing the dried mixed material, lubricant and antioxidant to obtain a mixed material; S3: Molding the mixed material to obtain a polyoxymethylene composite material.

[0016] Furthermore, the drying in step S1 is performed under vacuum conditions; preferably, the drying temperature is 70-80° C.; preferably, the drying time is 6-8 hours.

[0017] Furthermore, the melt mixing operation in step S2 is carried out in a twin-screw extruder, including feeding the dried mixed material into a feeder and extruding and granulating it in sequence through a feeding section, a melting section and a shearing section to obtain a mixed material; preferably, the temperature of the feeding section is 170-175°C, and the temperature of the melting section is 195-200°C; preferably, the feeder speed is 20-40r / min, and the screw speed is 150-300r / min; preferably, the particle size ratio of the granulation is 32-40.

[0018] Furthermore, the molding pressure is 15-20 MPa; preferably, the molding time is 5-7 min.

[0019] By using the polyoxymethylene composite material and the preparation method thereof provided by the present invention, the obtained polyoxymethylene composite material has a reduced friction coefficient, reduced wear, and significantly improved wear resistance, which is beneficial to the long-term use of the material, thereby improving the energy utilization efficiency and helping to save energy. In addition, based on the excellent performance of the polyoxymethylene composite material, it can also be applied to special fields with high requirements for materials, such as precision transmission parts manufacturing. DETAILED DESCRIPTION

[0020] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.

[0021] As described in the background technology section, polyoxymethylene (POM) has higher mechanical properties than other plastics, but relying solely on the inherent wear resistance of pure POM resin will result in a large amount of wear on the material, which is insufficient for long-term use in production and life. At the same time, the polyoxymethylene composite materials in the prior art also have problems such as high friction coefficient, large amount of wear, and insufficient wear resistance during use, and cannot meet the use of some special occasions with high requirements for material performance.

[0022] In order to solve the above problems, the present invention proposes a polyoxymethylene composite material, which includes the following components by weight: 70-95 parts of polyoxymethylene, 1-10 parts of polytetrafluoroethylene powder, 1-10 parts of glass fiber, 1-7 parts of polyethylene glycol, 0.5-1 part of antioxidant, and 0.5-2 parts of lubricant; wherein the weight average molecular weight of the polyethylene glycol is 5000-6000.

[0023] As a widely used engineering plastic, polyoxymethylene has extremely high strength and rigidity, and also has excellent properties such as good self-lubrication, corrosion resistance and dimensional stability. The present invention uses polyoxymethylene as a base, adds polytetrafluoroethylene powder, glass fiber, polyethylene glycol, antioxidant and lubricant to polyoxymethylene, and strictly controls each component in a certain proportion, so that each component works synergistically, and can better play their respective roles, thereby achieving the effect of comprehensively improving the performance of the polyoxymethylene composite material.

[0024] Specifically, the polyoxymethylene composite material described in the present application includes a variety of components, and the functions of various components in the polyoxymethylene composite material are not the same. Adding polytetrafluoroethylene powder can improve the friction performance of the polyoxymethylene composite material, and adding glass fiber can utilize its advantages of good rigidity, strength and thermal conductivity, while improving the bonding force of each component under the melting action, it can also improve the mechanical material properties and wear resistance of the polyoxymethylene composite material. Further, polyethylene glycol, antioxidant and lubricant are added, and these components and polyoxymethylene, polytetrafluoroethylene powder and glass fiber work synergistically to modify the polyoxymethylene together, so that the obtained polyoxymethylene composite material has good mechanical properties, and can also better reduce the friction coefficient of the composite material, reduce the amount of wear, and improve its wear resistance.

[0025] In particular, the present invention adds polyethylene glycol with a weight average molecular weight of 5000 to 6000 to the polyoxymethylene composite material. Polyethylene glycol is a chain polymer containing a large number of oxygen atoms and hydrogen atoms in the molecule. This structure makes polyethylene glycol have excellent properties such as good compatibility, dispersibility and adhesion. However, the difference in the weight average molecular weight of polyethylene glycol will lead to a large difference in its performance. After a lot of research, the inventor creatively found that adding polyethylene glycol with a weight average molecular weight in the range of 5000 to 6000 to the polyoxymethylene composite material, especially in combination with the use of components such as polytetrafluoroethylene and glass fiber, can better improve the effect of the polyoxymethylene composite material. After analysis, the above-mentioned polyethylene glycol plays the following roles in the polyoxymethylene composite material: first, polyethylene glycol can be used as a lubricant to synergistically modify polyoxymethylene with components such as polytetrafluoroethylene powder and glass fiber; second, the addition of polyethylene glycol can improve the toughness of the polyoxymethylene composite material, so that the resulting composite material has a better effect; third, the added polyethylene glycol can also be used as a dispersant to improve the uniform dispersion of components such as tetrafluoroethylene powder, glass fiber, and antioxidant, which helps to improve the comprehensive performance of the composite material. In particular, only when the weight average molecular weight of polyethylene glycol is within the range of 5000 to 6000, the resulting polyoxymethylene composite material will achieve better results. This is because when the molecular weight of polyethylene glycol is large, the plasticizing efficiency of polyethylene glycol decreases, and its lubricity, dispersibility and other properties will also decrease, and it cannot play a role in better improving the performance of the polyoxymethylene composite material. Preferably, the effective component of polyethylene glycol is 99% by mass, and the above effect is better.

[0026] In summary, the material proposed in the present invention includes a composite material of polyoxymethylene, polytetrafluoroethylene powder, glass fiber, polyethylene glycol, an antioxidant, and a lubricant, and the polyoxymethylene composite material obtained by strictly controlling their proportions has the advantages of low friction coefficient, low wear, high wear resistance, etc.; in particular, by controlling the weight average molecular weight of the polyethylene glycol within the range of 5000 to 6000, the relevant properties of the obtained polyoxymethylene composite material can be further improved.

[0027] In order to better improve the performance of the polyoxymethylene composite material, in a preferred embodiment, the polyoxymethylene composite material includes the following components by weight: 85-95 parts of polyoxymethylene, 1-5 parts of polytetrafluoroethylene powder, 1-5 parts of glass fiber, 1-3 parts of polyethylene glycol, 0.5-1 part of antioxidant, and 1-2 parts of lubricant. In the process of improving the performance of the polyoxymethylene composite material, the proportion of each component has a great influence on the mechanical strength, friction resistance and wear resistance of the polyoxymethylene composite material, especially on the comprehensive synergistic effect of each component. Controlling the proportion of each component within the above range can better achieve the purpose of improving the comprehensive performance of the polyoxymethylene composite material.

[0028] Further, the polyoxymethylene composite material includes the following components, by weight: 91 parts of polyoxymethylene, 3 parts of polytetrafluoroethylene powder, 1 part of glass fiber, 3 parts of polyethylene glycol, 0.5 parts of antioxidant, and 1.5 parts of lubricant, and the weight average molecular weight of polyethylene glycol is 6000; or, the polyoxymethylene composite material includes the following components, by weight: 91 parts of polyoxymethylene, 4 parts of polytetrafluoroethylene powder, 1 part of glass fiber, 3 parts of polyethylene glycol, 0.5 parts of antioxidant, and 0.5 parts of lubricant, and the weight average molecular weight of polyethylene glycol is 6000; or, the polyoxymethylene composite material includes the following components, by weight: 89.5 parts of polyoxymethylene, 4 parts of polytetrafluoroethylene powder, 2 parts of glass fiber, 2 parts of polyethylene glycol, 0.5 parts of antioxidant, and 2 parts of lubricant, and the weight average molecular weight of polyethylene glycol is 5000. When the above components are controlled within the above specific proportions, polyethylene glycol can achieve better synergistic effects with the various components, and the resulting polyoxymethylene composite material has better performance.

[0029] In a preferred embodiment, the polyoxymethylene is copolymer polyoxymethylene. Copolymer polyoxymethylene in polyoxymethylene has the advantages of good thermal stability, chemical stability, processability, etc. As the base material of polyoxymethylene composite material, it is compounded with various materials, which is more conducive to improving its wear resistance, reducing friction coefficient and wear while improving the mechanical properties of the obtained polyoxymethylene composite material. Preferably, the brand of copolymer polyoxymethylene is selected as at least one of MC90, MC270, and MC140, and when the melt flow rate of the above copolymer polyoxymethylene at 190°C is 9 to 27g / 10min, the comprehensive performance of the polyoxymethylene composite material prepared under this parameter is better.

[0030] In a preferred embodiment, the particle size of the polytetrafluoroethylene powder is 5 to 10 μm. The polytetrafluoroethylene powder plays a role in improving the mechanical properties and friction properties in the polyoxymethylene composite material. When the particle size of the polytetrafluoroethylene powder is small, it is conducive to better mixing with other substances in the component. When the particle size of the polytetrafluoroethylene powder is 5 to 10 μm, a good mixing effect can be achieved. Preferably, when the melt flow rate of the polytetrafluoroethylene powder in the component at 350°C is 5 to 6 g / 10 min, the polytetrafluoroethylene powder under this parameter can play a better role in the polyoxymethylene composite material.

[0031] In a preferred embodiment, the fiber length of the glass fiber is 5 to 20 mm and the diameter is 9 to 13 μm. Glass fiber is a commonly used reinforcing material. Adding glass fiber to polyoxymethylene composite materials can improve the bonding force between the components on the one hand, and on the other hand, it can also help improve the mechanical properties of the composite material, and synergize with other components in the composite material to further improve the comprehensive performance of the polyoxymethylene composite material. When the fiber length of the glass fiber is 5 to 20 mm and the diameter is 9 to 13 μm, it can be better integrated with the various components in the composite material. Preferably, the density of the glass fiber is 2.6 to 2.7 g / cm 3 The glass fiber under this parameter can play a better role when combined with the various components and the corresponding component ratios in the present invention.

[0032] In a preferred embodiment, the antioxidant is a hindered phenol antioxidant; preferably, the hindered phenol antioxidant is antioxidant 1010; preferably, the lubricant is silicone oil and / or mineral oil. When preparing the polyoxymethylene composite material, an antioxidant needs to be added. As a common type of oxidant, hindered phenol antioxidants have a relatively good antioxidant effect. Antioxidant 1010 is one of the hindered phenol antioxidants, composed of pentaerythritol tetrakis(methyl-β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate), which can better help improve the comprehensive performance of the polyoxymethylene composite material. The lubricant can be evenly distributed in the non-continuous micropores of the polyoxymethylene composite material in the polyoxymethylene composite material, thereby making the polyoxymethylene composite material have better rigidity and creep resistance, and can also effectively help the mixing of the various components, so that the various components in the polyoxymethylene composite material can work synergistically, and have a better improvement effect on the improvement of the comprehensive performance of the composite material.

[0033] According to another aspect of the present invention, a method for preparing a polyformaldehyde composite material is also provided, and the preparation method comprises the following steps S1: mixing and drying polyformaldehyde, polytetrafluoroethylene powder, glass fiber, polyethylene glycol, and an antioxidant to obtain a dried mixture; S2: melt-mixing the dried mixture with a lubricant and an antioxidant to obtain a mixture; S3: molding the mixture to obtain a polyformaldehyde composite material.

[0034] Specifically, in the preparation method of the polyformaldehyde composite material, polyformaldehyde, polytetrafluoroethylene powder, glass fiber, polyethylene glycol, and antioxidant are first mixed and dried at a certain temperature to remove a small amount of water in each component, so as to prepare for the subsequent melt mixing step. Then the dried mixture and lubricant are melted to obtain a mixed material. The operation of this step is conducive to fully mixing and melting the various components in the polyformaldehyde composite material. Finally, the obtained mixed material is molded to obtain the polyformaldehyde composite material. The preparation of the polyformaldehyde composite material is conducive to the mixing of the various components. The proportion of the components is controlled within a suitable range, so that the obtained polyformaldehyde composite material can be further improved in terms of mechanical properties, friction coefficient, wear amount, and wear resistance.

[0035] In a preferred embodiment, the drying in step S1 is carried out under vacuum conditions. The vacuum oxygen-free conditions will enable the components to better remove moisture from the components and trace oxygen contained in the pores of the component materials during the drying process, providing a basis for the fusion of the components in the subsequent steps. Preferably, the drying temperature is 70-80°C; preferably, the drying time is 6-8h. When the drying temperature and drying time are controlled within the above range, good results can be achieved.

[0036] In a preferred embodiment, the melt mixing operation in step S2 is carried out in a twin-screw extruder, including putting the dried mixed material into a feeder and extruding and granulating through a feed section, a melting section and a shearing section to obtain the above-mentioned mixed material. Compared with a single screw extruder, a twin-screw extruder has a better mixing effect, and the various components in the obtained composite material can be mixed more evenly. In addition, the process of mixing using a twin-screw extruder includes putting the dried mixed material into a feeder and then extruding and granulating through three stages of a feed section, a melting section and a shearing section. First, the mixed material will be preliminarily heated in the feeding stage, the mixed material will be preliminarily melt mixed, and then further heated and mixed in the melting stage so that the various components in the composite material can be better melted, and finally the mixed and melted mixture will be subjected to extrusion and granulation in the shearing section to obtain a mixed material. Preferably, the temperature of the feeding section is 170-175°C, and the temperature of the melting section is 195-200°C; preferably, the speed of the feeder is 20-40r / min, and the speed of the screw is 150-300r / min; preferably, the particle size ratio of granulation is 32-40. When the various parameters in the above process are controlled within the above range, a better mixing effect can be achieved.

[0037] In a preferred embodiment, the molding pressure is 15-20 MPa; preferably, the molding time is 5-7 min. Molding is a necessary operation in the preparation of composite materials, and the above conditions have better molding effects.

[0038] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.

[0039] It should be further explained below that the melt flow rate of copolymer polyoxymethylene is a parameter under the condition of a temperature of 190°C, and the melt flow rate of polytetrafluoroethylene powder is a parameter under the condition of a temperature of 350°C.

[0040] Example 1

[0041] The polyoxymethylene composite material comprises the following components in parts by weight:

[0042] Components Weight parts (parts) Component parameters Polyoxymethylene copolymer 91 Melt flow rate: 9g / 10min Polytetrafluoroethylene powder 3 Particle size is 5μm, melt flow rate is 5g / 10min Fiberglass 1 <![CDATA[Length is 5 mm, diameter is 9 μm, density is 2.6 g / cm 3 > Polyethylene glycol 3 The weight average molecular weight is 6000 Antioxidant 1010 0.5 / Silicone oil 1.5 /

[0043] The preparation steps of polyoxymethylene composite materials are as follows:

[0044] Step 1: Mix copolymer polyoxymethylene, polytetrafluoroethylene powder, glass fiber and polyethylene glycol and dry them under vacuum at 80° C. for 6 hours to obtain a dried mixture;

[0045] Step 2: The dried mixed material, silicone oil and antioxidant 1010 are mixed and put into the feeder of the twin-screw extruder, and extruded and granulated through the feeding section, melting section and shearing section in sequence to obtain a mixed material. The feeder speed is 40r / min, the screw speed is 150r / min, the temperature of the feeding section is 170°C, the temperature of the melting section is 195°C, and the particle size ratio of the extrusion granulation is 40.

[0046] Step 3: The mixed material is molded at 15 MPa for 7 minutes to obtain a polyoxymethylene composite material.

[0047] Example 2

[0048] The polyoxymethylene composite material comprises the following components in parts by weight:

[0049] Components Weight parts (parts) Component parameters Polyoxymethylene copolymer 91 Melt flow rate: 14g / 10min Polytetrafluoroethylene powder 4 Particle size is 5μm, melt flow rate is 5g / 10min Fiberglass 1 <![CDATA[Length is 5 mm, diameter is 9 μm, density is 2.6 g / cm 3 > Polyethylene glycol 3 The weight average molecular weight is 6000 Antioxidant 1010 0.5 / Mineral oil 0.5 /

[0050] The preparation steps of polyoxymethylene composite materials are as follows:

[0051] Step 1: Mix polyoxymethylene, polytetrafluoroethylene powder, glass fiber and polyethylene glycol and dry them at 70° C. for 8 hours to obtain a dried mixture;

[0052] Step 2: The dried mixed material, lubricant and antioxidant are mixed and fed into the feeder of a twin-screw extruder, and extruded and granulated through a feeding section, a melting section and a shearing section to obtain the mixed material. The feeder speed is 20 r / min, the screw speed is 300 r / min, the feeding section temperature is 175°C, the melting section temperature is 200°C, and the extrusion granulation particle size ratio is 32.

[0053] Step 3: The above-mentioned mixture is molded at 20 MPa for 5 minutes to obtain a polyoxymethylene composite material.

[0054] Example 3

[0055] The polyoxymethylene composite material comprises the following components in parts by weight:

[0056]

[0057]

[0058] The preparation steps of polyoxymethylene composite materials are as follows:

[0059] Step 1: Mix polyoxymethylene, polytetrafluoroethylene powder, glass fiber and polyethylene glycol and dry them at 70° C. for 8 hours to obtain a dried mixture;

[0060] Step 2: The dried mixed material, lubricant and antioxidant are mixed and put into the feeder of the twin-screw extruder, and extruded and granulated through the feeding section, melting section and shearing section to obtain the mixed material. The feeder speed is 40r / min, the screw speed is 300r / min, the temperature of the feeding section is 170°C, the temperature of the melting section is 195°C, and the particle size ratio of the extrusion granulation is 32.

[0061] Step 3: The mixed material is molded at 20 MPa for 7 minutes to obtain a polyoxymethylene composite material.

[0062] Example 4

[0063] The polyoxymethylene composite material comprises the following components in parts by weight:

[0064] Components Weight parts (parts) Component parameters Polyoxymethylene copolymer 70 Melt flow rate: 14g / 10min Polytetrafluoroethylene powder 10 Particle size is 10μm, melt flow rate is 6g / 10min Fiberglass 10 <![CDATA[Length is 5 mm, diameter is 13 μm, density is 2.7 g / cm 3 > Polyethylene glycol 7 The weight average molecular weight is 6000 Antioxidant 1010 1 / Silicone oil 2 /

[0065] The preparation steps of polyoxymethylene composite materials are as follows:

[0066] The preparation steps of polyoxymethylene composite materials are as follows:

[0067] Step 1: Mix polyoxymethylene, polytetrafluoroethylene powder, glass fiber and polyethylene glycol and dry them at 70° C. for 8 hours to obtain a dried mixture;

[0068] Step 2: The dried mixed material, lubricant and antioxidant are mixed and put into the feeder of the twin-screw extruder, and extruded and granulated through the feeding section, melting section and shearing section to obtain the mixed material. The feeder speed is 20r / min, the screw speed is 300r / min, the feeding section temperature is 170°C, the melting section temperature is 195°C, and the particle size ratio of the extrusion granulation is 32.

[0069] Step 3: The mixed material is molded at 20 MPa for 7 minutes to obtain a polyoxymethylene composite material.

[0070] Example 5

[0071] The polyoxymethylene composite material comprises the following components in parts by weight:

[0072] Components Weight parts (parts) Component parameters Polyoxymethylene copolymer 95 Melt flow rate: 14g / 10min Polytetrafluoroethylene powder 1 Particle size is 5μm, melt flow rate is 5g / 10min Fiberglass 1 <![CDATA[Length is 20 mm, diameter is 9 μm, density is 2.7 g / cm 3 > Polyethylene glycol 1 The weight average molecular weight is 6000 Antioxidant 1010 0.5 / Silicone oil 0.5 /

[0073] The preparation steps of polyoxymethylene composite materials are as follows:

[0074] Step 1: Mix polyoxymethylene, polytetrafluoroethylene powder, glass fiber and polyethylene glycol and dry them at 70° C. for 8 hours to obtain a dried mixture;

[0075] Step 2: The dried mixed material, lubricant and antioxidant are mixed and put into the feeder of the twin-screw extruder, and extruded and granulated through the feeding section, melting section and shearing section to obtain the mixed material. The feeder speed is 20r / min, the screw speed is 300r / min, the feeding section temperature is 170°C, the melting section temperature is 195°C, and the particle size ratio of the extrusion granulation is 32.

[0076] Step 3: The mixed material is molded at 20 MPa for 7 minutes to obtain a polyoxymethylene composite material.

[0077] Example 6

[0078] The polyoxymethylene composite material comprises the following components in parts by weight:

[0079]

[0080]

[0081] The preparation steps of polyoxymethylene composite materials are as follows:

[0082] Step 1: Mix copolymer polyoxymethylene, polytetrafluoroethylene powder, glass fiber and polyethylene glycol and dry them under vacuum at 80° C. for 6 hours to obtain a dried mixture;

[0083] Step 2: The dried mixed material, silicone oil and antioxidant 1010 are mixed and put into the feeder of the twin-screw extruder, and extruded and granulated through the feeding section, melting section and shearing section in sequence to obtain a mixed material. The feeder speed is 40r / min, the screw speed is 150r / min, the temperature of the feeding section is 170°C, the temperature of the melting section is 195°C, and the particle size ratio of the extrusion granulation is 40.

[0084] Step 3: The mixed material is molded at 15 MPa for 7 minutes to obtain a polyoxymethylene composite material.

[0085] Example 7

[0086] The difference from Example 1 is that the proportion of polyethylene glycol is increased to 10 parts.

[0087] The polyoxymethylene composite material comprises the following components in parts by weight:

[0088] Components Weight parts (parts) Component parameters Polyoxymethylene copolymer 91 Melt flow rate: 9g / 10min Polytetrafluoroethylene powder 3 Particle size is 5μm, melt flow rate is 5g / 10min Fiberglass 1 <![CDATA[Length is 5 mm, diameter is 9 μm, density is 2.6 g / cm 3 > Polyethylene glycol 10 The weight average molecular weight is 6000 Antioxidant 1010 0.5 / Silicone oil 1.5 /

[0089] The preparation steps of polyoxymethylene composite materials are as follows:

[0090] Step 1: Mix copolymer polyoxymethylene, polytetrafluoroethylene powder, glass fiber and polyethylene glycol and dry them under vacuum at 80° C. for 6 hours to obtain a dried mixture;

[0091] Step 2: The dried mixed material, silicone oil and antioxidant 1010 are mixed and put into the feeder of the twin-screw extruder, and extruded and granulated through the feeding section, melting section and shearing section in sequence to obtain a mixed material. The feeder speed is 40r / min, the screw speed is 150r / min, the temperature of the feeding section is 170°C, the temperature of the melting section is 195°C, and the particle size ratio of the extrusion granulation is 40.

[0092] Step 3: The mixed material is molded at 15 MPa for 7 minutes to obtain a polyoxymethylene composite material.

[0093] Example 8

[0094] The difference from Example 1 is that the proportion of polyethylene glycol is reduced to 0.5 parts.

[0095] The polyoxymethylene composite material comprises the following components in parts by weight:

[0096] Components Weight parts (parts) Component parameters Polyoxymethylene copolymer 91 Melt flow rate: 9g / 10min Polytetrafluoroethylene powder 3 Particle size is 5μm, melt flow rate is 5g / 10min Fiberglass 1 <![CDATA[Length is 5 mm, diameter is 9 μm, density is 2.6 g / cm 3 > Polyethylene glycol 0.5 The weight average molecular weight is 6000 Antioxidant 1010 0.5 / Silicone oil 1.5 /

[0097] The preparation steps of polyoxymethylene composite materials are as follows:

[0098] Step 1: Mix copolymer polyoxymethylene, polytetrafluoroethylene powder, glass fiber and polyethylene glycol and dry them under vacuum at 80° C. for 6 hours to obtain a dried mixture;

[0099] Step 2: The dried mixed material, silicone oil and antioxidant 1010 are mixed and put into the feeder of the twin-screw extruder, and extruded and granulated through the feeding section, melting section and shearing section in sequence to obtain a mixed material. The feeder speed is 40r / min, the screw speed is 150r / min, the temperature of the feeding section is 170°C, the temperature of the melting section is 195°C, and the particle size ratio of the extrusion granulation is 40.

[0100] Step 3: The mixed material is molded at 15 MPa for 7 minutes to obtain a polyoxymethylene composite material.

[0101] Example 9

[0102] The difference from Example 1 is that the molecular weight of polyethylene glycol is 9000, which is out of the range.

[0103] The polyoxymethylene composite material comprises the following components in parts by weight:

[0104]

[0105]

[0106] The preparation steps of polyoxymethylene composite materials are as follows:

[0107] Step 1: Mix copolymer polyoxymethylene, polytetrafluoroethylene powder, glass fiber and polyethylene glycol and dry them under vacuum at 80° C. for 6 hours to obtain a dried mixture;

[0108] Step 2: The dried mixed material, silicone oil and antioxidant 1010 are mixed and put into the feeder of the twin-screw extruder, and extruded and granulated through the feeding section, melting section and shearing section in sequence to obtain a mixed material. The feeder speed is 40r / min, the screw speed is 150r / min, the temperature of the feeding section is 170°C, the temperature of the melting section is 195°C, and the particle size ratio of the extrusion granulation is 40.

[0109] Step 3: The mixed material is molded at 15 MPa for 7 minutes to obtain a polyoxymethylene composite material.

[0110] Example 10

[0111] The polyoxymethylene composite material comprises the following components in parts by weight:

[0112] Components Weight parts (parts) Component parameters Polyoxymethylene copolymer 100 Melt flow rate: 9g / 10min Polytetrafluoroethylene powder 1 Particle size is 5μm, melt flow rate is 5g / 10min Fiberglass 0.5 <![CDATA[Length is 5 mm, diameter is 9 μm, density is 2.7 g / cm 3 > Polyethylene glycol 0.5 The weight average molecular weight is 6000 Antioxidant 1010 0.3 / Silicone oil 0.3 /

[0113] The preparation steps of polyoxymethylene composite materials are as follows:

[0114] Step 1: Mix copolymer polyoxymethylene, polytetrafluoroethylene powder, glass fiber and polyethylene glycol and dry them under vacuum at 80° C. for 8 hours to obtain a dried mixture;

[0115] Step 2: The dried mixed material, silicone oil and antioxidant 1010 are mixed and put into the feeder of the twin-screw extruder, and extruded and granulated through the feeding section, melting section and shearing section in sequence to obtain a mixed material. The feeder speed is 40r / min, the screw speed is 150r / min, the temperature of the feeding section is 170°C, the temperature of the melting section is 195°C, and the particle size ratio of the extrusion granulation is 40.

[0116] Step 3: The mixed material is molded at 15 MPa for 7 minutes to obtain a polyoxymethylene composite material.

[0117] Embodiment 11

[0118] The polyoxymethylene composite material comprises the following components in parts by weight:

[0119] Components Weight parts (parts) Component parameters Homopolymer polyoxymethylene 70 Melt flow rate: 14g / 10min Polytetrafluoroethylene powder 10 Particle size is 10μm, melt flow rate is 6g / 10min Fiberglass 10 <![CDATA[Length is 5 mm, diameter is 13 μm, density is 2.7 g / cm 3 > Polyethylene glycol 7 The weight average molecular weight is 6000 Antioxidant 1010 1 / Silicone oil 2 /

[0120] The preparation steps of polyoxymethylene composite materials are as follows:

[0121] The preparation steps of polyoxymethylene composite materials are as follows:

[0122] Step 1: Mix polyoxymethylene, polytetrafluoroethylene powder, glass fiber and polyethylene glycol and dry them at 70° C. for 8 hours to obtain a dried mixture;

[0123] Step 2: The dried mixed material, lubricant and antioxidant are mixed and put into the feeder of the twin-screw extruder, and extruded and granulated through the feeding section, melting section and shearing section to obtain the mixed material. The feeder speed is 20r / min, the screw speed is 300r / min, the feeding section temperature is 170°C, the melting section temperature is 195°C, and the particle size ratio of the extrusion granulation is 32.

[0124] Step 3: The mixed material is molded at 20 MPa for 7 minutes to obtain a polyoxymethylene composite material.

[0125] Comparative Example 1

[0126] The polyoxymethylene composite material comprises the following components in parts by weight:

[0127]

[0128]

[0129] The preparation steps of polyoxymethylene composite materials are as follows:

[0130] Step 1: drying the copolymerized polyoxymethylene under vacuum at 80°C for 8h;

[0131] Step 2: Mix the dried polyoxymethylene and antioxidant and put them into the feeder of the twin-screw extruder, and extrude and granulate them through the feeding section, melting section and shearing section to obtain a mixed material. The feeder speed is 40r / min, the screw speed is 150r / min, the temperature of the feeding section is 170°C, the temperature of the melting section is 195°C, and the particle size ratio of the extrusion granulation is 40.

[0132] Step 3: The mixed material is molded at 20 MPa for 7 minutes to obtain a polyoxymethylene composite material.

[0133] Comparative Example 2

[0134] The polyoxymethylene composite material comprises the following components in parts by weight:

[0135] Components Weight parts (parts) Component parameters Polyoxymethylene copolymer 94 Melt flow rate: 14g / 10min Polytetrafluoroethylene powder 5 The particle size is 5μm and the melt flow rate is 6g / 10min Antioxidant 1010 0.5 / Silicone oil 0.5 /

[0136] The preparation steps of polyoxymethylene composite materials are as follows:

[0137] Step 1: Mix the copolymer polyoxymethylene and polytetrafluoroethylene powder and dry them in vacuum at 80° C. for 8 hours to obtain a dried mixture;

[0138] Step 2: The dried mixed material, silicone oil and antioxidant 1010 are mixed and put into the feeder of the twin-screw extruder, and extruded and granulated through the feeding section, melting section and shearing section to obtain a mixed material. The feeder speed is 40r / min, the screw speed is 150r / min, the temperature of the feeding section is 170°C, the temperature of the melting section is 195°C, and the particle size ratio of the extrusion granulation is 35.

[0139] Step 3: The mixed material is molded at 15 MPa for 7 minutes to obtain a polyoxymethylene composite material.

[0140] Comparative Example 3

[0141] The polyoxymethylene composite material comprises the following components in parts by weight:

[0142]

[0143]

[0144] The preparation steps of polyoxymethylene composite materials are as follows:

[0145] Step 1: Mix the copolymer polyoxymethylene, polytetrafluoroethylene powder and glass fiber and dry them in vacuum at 80° C. for 8 hours to obtain a dried mixture;

[0146] Step 2: The dried mixed material, silicone oil and antioxidant 1010 are mixed and put into the feeder of the twin-screw extruder, and extruded and granulated through the feeding section, melting section and shearing section to obtain a mixed material. The feeder speed is 40r / min, the screw speed is 150r / min, the temperature of the feeding section is 170°C, the temperature of the melting section is 195°C, and the particle size ratio of the extrusion granulation is 35.

[0147] Step 3: The mixed material is molded at 15 MPa for 7 minutes to obtain a polyoxymethylene composite material.

[0148] Comparative Example 4

[0149] The polyoxymethylene composite material comprises the following components in parts by weight:

[0150] Components Weight parts (parts) Component parameters Polyoxymethylene copolymer 94 Melt flow rate: 14g / 10min Polytetrafluoroethylene powder 2 The particle size is 5μm and the melt flow rate is 6g / 10min Polyethylene glycol 3 The weight average molecular weight is 6000 Antioxidant 1010 0.5 / Silicone oil 0.5 /

[0151] The preparation steps of polyoxymethylene composite materials are as follows:

[0152] Step 1: Mix copolymer polyoxymethylene, polytetrafluoroethylene powder and polyethylene glycol and dry them in vacuum at 80° C. for 8 hours to obtain a dried mixture;

[0153] Step 2: The dried mixed material, silicone oil and antioxidant 1010 are mixed and put into the feeder of the twin-screw extruder, and extruded and granulated through the feeding section, melting section and shearing section to obtain a mixed material. The feeder speed is 40r / min, the screw speed is 150r / min, the temperature of the feeding section is 170°C, the temperature of the melting section is 195°C, and the particle size ratio of the extrusion granulation is 35.

[0154] Step 3: The mixed material is molded at 15 MPa for 7 minutes to obtain a polyoxymethylene composite material.

[0155] The friction and mechanical properties of the composite materials prepared in the above examples and comparative examples were tested, and the results are shown in Table 1. The test standards for friction and mechanical properties need to be further explained here:

[0156] (1) Friction performance test

[0157] According to GB / T3960, the wear amount and friction coefficient of the polyoxymethylene composite material were tested under the wear resistance test conditions of 2h of wear with a linear speed of 200r / min, a load of 25KJ, and a normal load of 500N.

[0158] (2) Mechanical properties test

[0159] Tensile properties: According to GB / T1040.2 standard, the tensile properties of polyoxymethylene composite materials were tested at a test speed of 50 mm / min;

[0160] Bending properties: The bending properties of polyoxymethylene composite materials were tested according to ASTM D790, with a test speed of 2 mm / min;

[0161] Notched impact strength properties: The notched impact strength of polyoxymethylene composites was tested according to ISO 180-1992 standard.

[0162] Table 1

[0163]

[0164]

[0165] In Examples 1 to 11, when the polyoxymethylene composite material is prepared by the preparation method described in the present application, by adding polyethylene glycol with a weight average molecular weight in the range of 5000 to 6000 and controlling the proportion of each component within a suitable range, the friction coefficient and wear amount of the obtained polyoxymethylene composite material are significantly reduced, and the mechanical properties, impact resistance and toughness can also be guaranteed to be within a suitable range. Among them, in Examples 1 to 6 and Example 11, when preparing the polyoxymethylene composite material, the proportion of each component is controlled within the preferred range described in the present invention, and the sliding friction coefficient of the obtained polyoxymethylene composite material is ≤0.20; the mass wear is ≤0.8mg, the tensile strength is ≥50.0MPa, the elongation at break is ≥20.0%, and the notched impact strength is ≥6.0kJ / m 2 , bending modulus ≥ 2000MPa, the polyoxymethylene product prepared by the present invention not only has high wear resistance and low friction coefficient characteristics, but also maintains the excellent mechanical properties of the polyoxymethylene product, and has good comprehensive performance. However, in Examples 7 to 10, the addition amount of polyethylene glycol is too much or too little, the molecular weight of the added polyethylene glycol is too large, or the proportion of each component is not within the protection range, which will affect the comprehensive performance of the polyoxymethylene composite material.

[0166] In Comparative Examples 1 to 4, only one or more of the components described in the present application were added when preparing the polyoxymethylene composite material. The friction coefficient and wear amount of the obtained polyoxymethylene composite material were relatively large, and the comprehensive performance was difficult to meet the higher requirements for the use standards of the polyoxymethylene composite material.

[0167] In summary, the prepared wear-resistant polyoxymethylene composite material not only has excellent wear resistance, but also has good mechanical properties, which is conducive to the long-term use of the material, can fully meet the actual use requirements of the material, and can also be used in special fields with high requirements for materials such as precision transmission parts manufacturing. And the preparation method is simple and easy to apply to production.

[0168] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A polyoxymethylene composite material, characterized in that: The polyoxymethylene composite material comprises the following components by weight: 70 to 95 parts of polyoxymethylene, 1 to 10 parts of polytetrafluoroethylene powder, 1 to 10 parts of glass fiber, 1 to 7 parts of polyethylene glycol, 0.5 to 1 part of antioxidant, and 0.5 to 2 parts of lubricant; wherein the weight average molecular weight of the polyethylene glycol is 5000 to 6000.

2. The polyoxymethylene composite material according to claim 1, characterized in that: The polyoxymethylene composite material comprises the following components by weight: 85-95 parts of the polyoxymethylene, 1-5 parts of the polytetrafluoroethylene powder, 1-5 parts of the glass fiber, 1-3 parts of the polyethylene glycol, 0.5-1 parts of the antioxidant, and 1-2 parts of the lubricant; Preferably, the polyoxymethylene composite material comprises the following components in parts by weight: 91 parts of the polyoxymethylene, 3 parts of the polytetrafluoroethylene powder, 1 part of the glass fiber, 3 parts of the polyethylene glycol, 0.5 parts of the antioxidant, and 1.5 parts of the lubricant, and the weight average molecular weight of the polyethylene glycol is 6000; or, The polyoxymethylene composite material comprises the following components by weight: 91 parts of polyoxymethylene, 4 parts of polytetrafluoroethylene powder, 1 part of glass fiber, 3 parts of polyethylene glycol, 0.5 parts of antioxidant, and 0.5 parts of lubricant, and the weight average molecular weight of the polyethylene glycol is 6000; or, The polyoxymethylene composite material comprises the following components by weight: 89.5 parts of the polyoxymethylene, 4 parts of the polytetrafluoroethylene powder, 2 parts of the glass fiber, 2 parts of the polyethylene glycol, 0.5 parts of the antioxidant, and 2 parts of the lubricant, and the weight average molecular weight of the polyethylene glycol is 5000.

3. The polyoxymethylene composite material according to claim 1, characterized in that: The polyoxymethylene is copolymer polyoxymethylene; Preferably, the melt flow rate of the copolymer polyoxymethylene at 190° C. is 9 to 27 g / 10 min; Further preferably, the brand of the copolymer polyoxymethylene is at least one of MC90, MC270 and MC140.

4. The polyoxymethylene composite material according to any one of claims 1 to 3, characterized in that: The particle size of the polytetrafluoroethylene powder is 5 to 10 μm; Preferably, the melt flow rate of the polytetrafluoroethylene powder at 350° C. is 5 to 6 g / 10 min.

5. The polyoxymethylene composite material according to any one of claims 1 to 3, characterized in that: The fiber length of the glass fiber is 5 to 20 mm and the diameter is 9 to 13 μm; Preferably, the density of the glass fiber is 2.6-2.7 g / cm 3 .

6. The polyoxymethylene composite material according to any one of claims 1 to 3, characterized in that: The antioxidant is a hindered phenol antioxidant; Preferably, the hindered phenol antioxidant is antioxidant 1010; Preferably, the lubricant is silicone oil and / or mineral oil.

7. A method for preparing the polyoxymethylene composite material according to any one of claims 1 to 6, characterized in that: The preparation method comprises the following steps: S1: Mixing and drying polyoxymethylene, polytetrafluoroethylene powder, glass fiber and polyethylene glycol to obtain a dried mixture; S2: Melting and mixing the dried mixed material, lubricant and antioxidant to obtain a mixed material; S3: molding the mixed material to obtain the polyoxymethylene composite material.

8. The method for preparing the polyoxymethylene composite material according to claim 7, characterized in that: The drying in step S1 is performed under vacuum conditions; Preferably, the drying temperature is 70-80°C; Preferably, the drying time is 6 to 8 hours.

9. The method for preparing the polyoxymethylene composite material according to claim 7, characterized in that: The melt mixing operation in step S2 is performed in a twin-screw extruder, including feeding the dried mixed material into a feeder and extruding and granulating the dried mixed material through a feeding section, a melting section and a shearing section in sequence to obtain the mixed material; Preferably, the temperature of the feeding section is 170-175°C, and the temperature of the melting section is 195-200°C; Preferably, the feeder speed is 20-40 r / min, and the screw speed is 150-300 r / min; Preferably, the particle size ratio of the granulation is 32-40.

10. The method for preparing the polyoxymethylene composite material according to any one of claims 7 to 9, characterized in that: The molding pressure is 15-20 MPa; Preferably, the molding time is 5 to 7 minutes.