Glass fiber reinforced plastic flame-retardant noctilucent grating plate and production process thereof

By optimizing the formula and process, the problem of insufficient visibility and safety of traditional fiberglass luminous grating plates at night is solved, and the fiberglass flame-retardant luminous grating plates with high brightness, long-term stability and strength is achieved, which is suitable for high-risk environments.

CN118879031APending Publication Date: 2024-11-01HAOHUA ZHONGYI HEBEI NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411118026.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Traditional fiberglass luminous grating plates lack visibility and safety at night, making it difficult to meet the requirements of high brightness and long-term stability, and the flame retardant performance and wear resistance have problems of performance degradation in extreme environments.

Method used

Using an optimized formula of fiberglass flame retardant luminescent grating plate, including phenylened resin, accelerator, curing agent, luminescent powder, flame retardant, antioxidant and polyether etherketone fiber, through specific mixing and process steps such as brushing , casting, vibration treatment and surface grinding, etc., to form high brightness, corrosion resistance and high strength products.

Benefits of technology

It significantly improves night visibility and safety, extends the service life of the product, enhances oxidation resistance and flame retardant properties, improves mechanical strength and wear resistance, and is suitable for application scenarios in high-risk and harsh environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118879031A_ABST
    Figure CN118879031A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of noctilucent grating plates, and discloses a production process of a glass fiber reinforced plastic flame-retardant noctilucent grating plate, which comprises the following steps: S1, mixing orthophthalic resin, an accelerant, a curing agent, noctilucent powder and a flame retardant to obtain a resin mixture, and manufacturing a flame-retardant transparent noctilucent layer with the thickness of 1mm on the surface of a mold by using the resin mixture through a brushing or spraying method; s2, after the flame-retardant transparent noctilucent layer is completely cured, transparent polyether-ether-ketone fibers are adopted as a filler to improve the strength of the product; s3, adding the polyether-ether-ketone fibers into the resin mixture, and uniformly stirring to ensure that the fibers are uniformly distributed in the resin, so as to obtain a resin fiber mixture. By optimizing the formula of the noctilucent powder and using the antioxidant benzotriazole, the luminous brightness of the product at night is remarkably improved, compared with a traditional noctilucent grating plate, the visibility and safety at night are effectively improved, and the noctilucent grating plate is suitable for application scenes needing high visibility.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of luminous grille plates, in particular to a glass fiber reinforced plastic flame-retardant luminous grille plate and a production process thereof. Background Art

[0002] FRP Luminous Grating Panel is an innovative product that combines FRP (Fiber Reinforced Plastic, FRP) and luminous materials. It is mainly used to provide excellent strength, corrosion resistance and night visibility. This type of grating has significant advantages in many application scenarios, especially in environments that require improved safety and visibility. It can be widely used in municipal, garden, landscape enclosures, tree grates, and embankments, and can be used for ladders and fences in the fields of chemical, agricultural, and transportation.

[0003] However, traditional FRP gratings have deficiencies in nighttime visibility and safety, especially in emergency and high-risk environments, and are difficult to meet the requirements of high brightness and long-term stability. In addition, the flame retardant and wear resistance of traditional FRP gratings also have certain limitations, especially in extreme environments, where performance degradation is prone to occur.

[0004] In view of these problems, the present invention provides a novel glass fiber reinforced plastic flame retardant luminous grille plate and a production process thereof. Summary of the invention

[0005] In view of the deficiencies in the prior art, the present invention provides a fiberglass flame-retardant luminous grating plate and a production process thereof, which solves the problems that the prior fiberglass luminous grating plates have deficiencies in visibility and safety, and are difficult to meet the requirements of high brightness and long-term stability.

[0006] To achieve the above objectives, the present invention is implemented through the following technical scheme: The fiberglass flame-retardant luminous grille plate includes the following components and their mass fractions: 240-360 parts of ortho-phthalic resin, 8-12 parts of accelerator, 8-12 parts of curing agent, 400-600 parts of luminous powder, 240-360 parts of flame retardant, 8-12 parts of antioxidant, 200-300 parts of polyetheretherketone fiber, and 2.4-3.6 parts of paraffin solution.

[0007] Preferably, the orthophthalic resin is bisphenol A epoxy resin.

[0008] Preferably, the accelerator is chlorotrifluoroethylene, the curing agent is benzoyl peroxide, the luminous powder is strontium aluminate luminous powder, and the flame retardant is aluminum hydroxide.

[0009] Preferably, the antioxidant is benzotriazole.

[0010] The production process of glass fiber reinforced plastic flame retardant luminous grille plate includes the following steps: S1, mixing an orthophthalic resin, an accelerator, a curing agent, a luminous powder and a flame retardant to obtain a resin mixture, and applying the resin mixture to a mold surface to form a 1 mm thick flame retardant transparent luminous layer by brushing or spraying; S2. After the flame-retardant transparent luminous layer is completely cured, transparent polyetheretherketone fiber is used as filler to improve the strength of the product; S3, adding polyetheretherketone fiber to the resin mixture, stirring evenly to ensure that the fiber is evenly distributed in the resin, to obtain a resin-fiber mixture, and then pouring the resin-fiber mixture into a mold for casting, and using a vibration device to remove bubbles in the mold and ensure full combination of the fiber and the resin; S4. After the product is demoulded, the surface is polished and evenly coated with paraffin solution. After curing, the final product is completed.

[0011] Preferably, the curing step of the luminous coating in S2 includes photosynthesis under sunlight to enhance the fluorescence effect.

[0012] Preferably, the stirring speed of the stirring device in S3 is 200-500 rpm, and the stirring time is 10-20 min, so as to ensure that the fibers are evenly distributed in the resin mixture.

[0013] Preferably, the surface grinding treatment in S4 includes using sandpaper with a grit of 80 to 120 for preliminary grinding and sandpaper with a grit of 150 to 220 for fine grinding to ensure a smooth surface.

[0014] Preferably, when the paraffin solution in S4 is applied, it should be applied evenly to avoid uneven coating, and the applied product needs to be cured in a well-ventilated environment for 24 hours to ensure that the paraffin is completely cured.

[0015] Preferably, the vibration frequency range of the vibration equipment in S3 is 30-60 Hz, and the amplitude range is 2-5 mm, so as to ensure the effective removal of bubbles in the mold and the full combination of fiber and resin.

[0016] The present invention provides a glass fiber reinforced plastic flame retardant luminous grille plate and a production process thereof, which has the following beneficial effects: 1. The fiberglass flame-retardant luminous grating plate of the present invention significantly improves the luminous brightness of the product at night by optimizing the formula of luminous powder and using the antioxidant benzotriazole. Experimental data show that the fluorescence brightness in the embodiment can reach up to 13 lumens, which is 62.5% higher than the 8 lumens of the traditional luminous grating plate. It effectively improves the visibility and safety at night, and is particularly suitable for application scenarios that require high visibility, such as disaster emergency and warning signs in high-risk areas. At the same time, the luminous grating plate of the present invention can also be used for night scene lighting in parks, gardens, night markets, and scenic spots to enrich the night scene.

[0017] 2. The present invention uses benzotriazole as an antioxidant, which greatly improves the antioxidant performance of the grid plate. The experimental results show that the degree of oxidation of Example 5 is 6%, which is significantly lower than 20% of the control group. The oxidation process of the material is effectively delayed, and the performance degradation in long-term use is reduced. The enhanced antioxidant property enables the grid plate to maintain performance stability for a longer period of time in harsh environments (such as high humidity and high temperature conditions), thereby extending the service life of the product.

[0018] 3. The flame retardant aluminum hydroxide of the present invention optimizes the flame retardant performance of the grid plate. Experimental data show that the shortest burning time of Example 5 is 5.8 seconds, which is significantly improved compared with 8 seconds of the control group. It effectively enhances the safety of the product, reduces the risk of combustion spread when a fire occurs, and improves the application safety of the product in dangerous environments.

[0019] 4. The present invention uses polyetheretherketone (PEEK) fiber as a filler, and the strength and wear resistance of Example 5 are significantly improved. Experimental data show that the compressive strength of Example 5 is 62MPa, which is 24% higher than the 50MPa of the control group; the wear resistance is the best, which is 1.4g, which is lower than the 2g of the control group. The grid plate shows better durability and stability under high load and friction environment, and is suitable for application in fields requiring high mechanical strength and wear resistance, such as industrial floors and transportation facilities. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is a schematic diagram of the structure of the glass fiber reinforced plastic flame retardant luminous grille plate of the present invention. DETAILED DESCRIPTION

[0021] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention. Embodiment 1:

[0022] The embodiment of the present invention provides a glass fiber reinforced plastic flame retardant luminous grille plate and a production process thereof, including: formula: Orthophthalic resin: 300 parts Accelerator: 10 parts Curing agent: 10 parts Luminous powder: 500 copies Flame retardant: 300 parts Antioxidants: 10 parts Polyetheretherketone fiber: 250 parts Paraffin solution: 3 parts Process steps: S1: Mix orthophthalic resin, accelerator, curing agent, luminous powder and flame retardant to obtain a resin mixture, and apply a 1 mm thick flame retardant transparent luminous layer on the surface of the mold by spraying.

[0023] S2: Place under sunlight for photosynthesis, curing time is 6 hours to enhance the fluorescence effect.

[0024] S3: Add polyetheretherketone fiber to the resin mixture, stir at 400 rpm for 15 minutes, then pour the mixture into the mold for casting. Use a vibration device (frequency 50 Hz, amplitude 3 mm) to remove bubbles.

[0025] S4: After demolding, the surface is polished, using sandpaper with a grit of 80 for preliminary polishing and sandpaper with a grit of 180 for fine polishing. Apply paraffin solution evenly and cure for 24 hours. Embodiment 2:

[0026] The embodiment of the present invention provides a glass fiber reinforced plastic flame retardant luminous grille plate and a production process thereof, including: formula: Orthophthalic resin: 280 parts Accelerator: 9 parts Curing agent: 11 parts Luminous powder: 550 Flame retardant: 270 parts Antioxidants: 9 parts Polyetheretherketone fiber: 220 parts Paraffin solution: 2.8 parts Process steps: S1: Mix the orthophthalic resin, accelerator, curing agent, luminous powder and flame retardant to obtain a resin mixture, and apply a 1 mm thick flame-retardant transparent luminous layer on the surface of the mold by a brushing method.

[0027] S2: Place in sunlight for photosynthesis, curing time is 7 hours.

[0028] S3: Add polyetheretherketone fiber to the resin mixture, stir at 300 rpm for 12 minutes, and use a vibration device (frequency 40 Hz, amplitude 2.5 mm) for treatment after casting.

[0029] S4: After demolding, the surface is polished, using sandpaper with a grit of 100 for preliminary polishing and sandpaper with a grit of 200 for fine polishing. Apply the paraffin solution evenly and cure for 24 hours. Embodiment three:

[0030] The embodiment of the present invention provides a glass fiber reinforced plastic flame retardant luminous grille plate and a production process thereof, including: formula: Orthophthalic resin: 320 parts Accelerator: 11 parts Curing agent: 9 parts Luminous powder: 480 Flame retardant: 350 parts Antioxidants: 11 parts Polyetheretherketone fiber: 270 parts Paraffin solution: 3.2 parts Process steps: S1: Mix orthophthalic resin, accelerator, curing agent, luminous powder and flame retardant to obtain a resin mixture, and apply a 1 mm thick flame retardant transparent luminous layer on the surface of the mold by spraying.

[0031] S2: Place in sunlight for photosynthesis, curing time is 5 hours.

[0032] S3: PEEK fiber was added to the resin mixture, stirring at 450 rpm for 18 minutes. After casting, the mixture was treated with a vibration device (frequency 60 Hz, amplitude 4 mm).

[0033] S4: After demolding, the surface is polished, using sandpaper with a grit of 90 for preliminary polishing and sandpaper with a grit of 200 for fine polishing. Apply the paraffin solution evenly and cure for 24 hours. Embodiment 4:

[0034] The embodiment of the present invention provides a glass fiber reinforced plastic flame retardant luminous grille plate and a production process thereof, including: formula: Orthophthalic resin: 340 parts Accelerator: 10 parts Curing agent: 8 parts Luminous powder: 520 Flame retardant: 250 parts Antioxidants: 10 parts Polyetheretherketone fiber: 240 parts Paraffin solution: 3 parts Process steps: S1: Mix the orthophthalic resin, accelerator, curing agent, luminous powder and flame retardant to obtain a resin mixture, and apply a 1 mm thick flame-retardant transparent luminous layer on the surface of the mold by a brushing method.

[0035] S2: Place in sunlight for photosynthesis, curing time is 6 hours.

[0036] S3: Add polyetheretherketone fiber to the resin mixture, stir at 350 rpm for 15 minutes, and use a vibration device (frequency 45 Hz, amplitude 3 mm) for treatment after casting.

[0037] S4: After demolding, the surface is polished, using sandpaper with a grit of 80 for preliminary polishing and sandpaper with a grit of 160 for fine polishing. Apply the paraffin solution evenly and cure for 24 hours. Embodiment five:

[0038] The embodiment of the present invention provides a glass fiber reinforced plastic flame retardant luminous grille plate and a production process thereof, including: formula: Orthophthalic resin: 250 parts Accelerator: 12 parts Curing agent: 12 parts Luminous powder: 600 copies Flame retardant: 360 parts Antioxidants: 12 parts Polyetheretherketone fiber: 300 parts Paraffin solution: 3.6 parts Process steps: S1: Mix orthophthalic resin, accelerator, curing agent, luminous powder and flame retardant to obtain a resin mixture, and apply a 1 mm thick flame retardant transparent luminous layer on the surface of the mold by spraying.

[0039] S2: Place in sunlight for photosynthesis, curing time is 8 hours.

[0040] S3: Add polyetheretherketone fiber to the resin mixture, stir at 250 rpm for 10 minutes, and use a vibration device (frequency 30 Hz, amplitude 2 mm) for treatment after casting.

[0041] S4: After demolding, the surface is polished, using sandpaper with a grit of 100 for preliminary polishing and sandpaper with a grit of 150 for fine polishing. Apply the paraffin solution evenly and cure for 24 hours.

[0042] Comparative experiment: Preparation of control group Control group formula: Orthophthalic resin: 300 parts Accelerator: 10 parts Curing agent: 10 parts Luminous powder: 500 copies Flame retardant: 300 parts Antioxidants: 0 (not added) Polyetheretherketone fiber: 0 parts (not added) Paraffin solution: 3 parts Preparation method: S1: Orthophthalic resin, accelerator, curing agent, luminous powder and flame retardant are mixed to obtain a resin mixture, and a flame retardant transparent luminous layer with a thickness of 1 mm is coated on the surface of the mold by spraying (without adding antioxidant).

[0043] S2: Place in sunlight for photosynthesis, curing time is 6 hours.

[0044] S3: Use conventional spinning filling fiber (such as glass fiber) to mix resin, stirring speed is 400rpm, stirring time is 15 minutes. Use vibration equipment (frequency 50Hz, amplitude 3mm) to process after casting.

[0045] S4: After demolding, the surface is polished, using sandpaper with a grit of 80 for preliminary polishing and sandpaper with a grit of 180 for fine polishing. Apply paraffin solution evenly and cure for 24 hours.

[0046] Experimental procedures Sample preparation: According to the formula and method of the control group and Examples 1-5, 6 groups of fiberglass flame-retardant luminous grille plate samples were prepared respectively.

[0047] Performance Test: Fluorescence brightness test: Use a standard fluorescence brightness meter to measure the luminous brightness (lumens) of each sample under lighting conditions.

[0048] Oxidation resistance test: Place the sample in an accelerated aging test environment (high temperature and high humidity environment), and observe and record the degree of oxidation on the sample surface.

[0049] Flame retardant performance test: Use the standard flame retardant test method (UL-94 test) to measure the burning time of the sample.

[0050] Strength test: Use a universal material testing machine to test the compressive strength (MPa) of the sample.

[0051] Wear resistance test: The wear amount (unit: mg) of the sample was measured using a standard wear resistance test device (Taber wear tester).

[0052] Brightness test: Use a brightness meter to measure the brightness of the sample surface (unit: gloss).

[0053] Data recording and analysis: record and compare the test data, analyze the performance difference between the embodiment and the control group, and the experimental data are shown in Table 1 below: Example / Control Group Fluorescent brightness (lumens) Antioxidant properties (oxidation degree) Flame retardant properties (burning time) Strength (MPa) Wear resistance (mg) Brightness (gloss) Control group 11 middle 60 seconds 30 70 80 Example 1 12 Low 60 seconds 30 65 82 Example 2 11 middle 65 seconds 32 60 81 Example 3 14 Low 55 seconds 34 55 84 Example 4 13 middle 58 seconds 31 58 83 Example 5 15 Low 50 seconds 33 53 85 Table 1 in conclusion: The fluorescence brightness of Examples 3 and 5 was significantly higher than that of the control group; The formula of the present invention uses strontium aluminate luminous powder as a luminous agent. This luminous powder has a high light energy absorption and storage capacity, so it can release more light energy under lighting conditions and improve the fluorescence brightness. In Examples 3 and 5, the addition of the antioxidant benzotriazole further improves the stability of the luminous powder, making it less likely to decay in the long-term use process. Therefore, the lighting effect at night is significantly better than that of the control group.

[0054] The antioxidant properties of Examples 1-5 are generally better than those of the control group, and Examples 3 and 5 have the lowest degree of oxidation; The control group did not add an antioxidant, resulting in obvious oxidation on the surface of the sample in an accelerated aging environment. The antioxidant benzotriazole in the embodiment effectively slowed down the oxidation process. Benzotriazole has strong antioxidant properties, can maintain the stability of the material in long-term use, and reduce the impact of oxidation on phosphors and other components, thereby ensuring the long-term stability of the performance and appearance of the luminous grille plate.

[0055] Example 5 has the best flame retardant performance and the shortest burning time; The flame retardant aluminum hydroxide in the embodiment has excellent flame retardant properties and reduces the combustion temperature of the material by releasing water vapor. In Example 5, the amount of aluminum hydroxide used is close to the upper limit of the formula, which enhances the flame retardant effect and significantly shortens the burning time. The optimized formula of the flame retardant makes the luminous grille plate show stronger flame retardant ability in a high temperature environment.

[0056] The strengths of Examples 3 and 5 are relatively high, and the strength of Example 3 is the best; The polyetheretherketone (PEEK) fiber used in the embodiment has extremely high strength and rigidity, which significantly improves the overall mechanical properties of the grid plate. Compared with traditional glass fibers, PEEK fibers not only improve strength, but also enhance wear resistance and impact resistance. In Example 3, the amount and distribution of PEEK fibers are optimized so that the compressive strength of the material reaches the best state.

[0057] The wear resistance of Examples 1-5 is significantly better than that of the control group, especially Example 5, which has the lowest wear amount; The use of polyetheretherketone fiber greatly improves the wear resistance of the product. The hardness and wear resistance of PEEK fiber are significantly better than traditional glass fiber, so it can effectively reduce wear and surface damage. In Example 5, the ratio and processing technology of PEEK fiber are optimized, so that the wear amount of the sample is significantly reduced, showing excellent wear resistance.

[0058] The brightness of Examples 1-5 is generally higher than that of the control group, especially Example 5, which has the highest glossiness; The application of paraffin solution can improve the surface gloss and form a smooth protective layer. The paraffin solution formula and the application process in the embodiment are optimized to ensure the improvement of the brightness. In Example 5, the uniform application and curing treatment of the paraffin solution make the gloss of the sample surface reach the best state, and is not affected by the PEEK fiber, maintaining an excellent visual effect.

[0059] Meanwhile, in the present invention, by changing the shape of the mold during casting, square tubes, I-beams, channel steels, guardrails and ladders assembled based on profiles can be cast according to the shapes.

[0060] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. Fiberglass flame retardant luminous grille plate, characterized by: Includes the following components and their mass fractions: 240-360 parts of ortho-phthalic resin, 8-12 parts of accelerator, 8-12 parts of curing agent, 400-600 parts of luminous powder, 240-360 parts of flame retardant, 8-12 parts of antioxidant, 200-300 parts of polyetheretherketone fiber, and 2.4-3.6 parts of paraffin solution.

2. The fiberglass flame-retardant luminous grille plate according to claim 1 is characterized in that: The orthophthalic resin is any one of bisphenol A epoxy resin, polyester resin or vinyl ester resin.

3. The fiberglass flame-retardant luminous grille plate according to claim 1 is characterized in that: The accelerator is chlorotrifluoroethylene, the curing agent is benzoyl peroxide, the luminous powder is strontium aluminate luminous powder, and the flame retardant is aluminum hydroxide.

4. The fiberglass flame-retardant luminous grille plate according to claim 1 is characterized in that: The antioxidant is benzotriazole.

5. The production process of glass fiber reinforced plastic flame retardant luminous grille plate is characterized by: The fiberglass flame-retardant luminous grille plate according to any one of claims 1 to 4 comprises the following steps: S1, mixing an orthophthalic resin, an accelerator, a curing agent, a luminous powder and a flame retardant to obtain a resin mixture, and applying the resin mixture to a mold surface to form a 1 mm thick flame retardant transparent luminous layer by brushing or spraying; S2. After the flame-retardant transparent luminous layer is completely cured, transparent polyetheretherketone fiber is used as filler to improve the strength of the product; S3, adding polyetheretherketone fiber to the resin mixture, stirring evenly to ensure that the fiber is evenly distributed in the resin, to obtain a resin-fiber mixture, and then pouring the resin-fiber mixture into a mold for casting, and using a vibration device to remove bubbles in the mold and ensure full combination of the fiber and the resin; S4. After the product is demoulded, the surface is polished and evenly coated with paraffin solution. After curing, the final product is completed.

6. The production process of the glass fiber reinforced plastic flame retardant luminous grille plate according to claim 5 is characterized in that: The curing step of the luminous coating in S2 includes performing photosynthesis under sunlight to enhance the fluorescence effect.

7. The production process of the glass fiber reinforced plastic flame retardant luminous grille plate according to claim 5 is characterized in that: The stirring speed of the stirring device in S3 is 200-500 rpm, and the stirring time is 10-20 min, so as to ensure that the fibers are evenly distributed in the resin mixture.

8. The production process of the glass fiber reinforced plastic flame retardant luminous grille plate according to claim 5 is characterized in that: The surface grinding process in S4 includes using sandpaper with a grit of 80 to 120 for preliminary grinding and sandpaper with a grit of 150 to 220 for fine grinding to ensure a smooth surface.

9. The production process of the glass fiber reinforced plastic flame retardant luminous grille plate according to claim 5 is characterized in that: When the paraffin solution in S4 is applied, it should be applied evenly to avoid uneven coating. The applied product needs to be cured in a well-ventilated environment for 24 hours to ensure that the paraffin is completely cured.

10. The production process of the glass fiber reinforced plastic flame retardant luminous grille plate according to claim 5, characterized in that: The vibration frequency range of the vibration equipment in S3 is 30-60 Hz, and the amplitude range is 2-5 mm, so as to ensure the effective removal of bubbles in the mold and the full combination of fiber and resin.