Elastic hollow glass bead as well as preparation method and application thereof

By forming a divinylbenzene modified polyurethane layer on the surface of hollow glass microbeads, the problem of high breakage rate of microbeads in new energy vehicles is solved, and the effect of lightweight sealant and good curing performance is achieved.

CN118879100APending Publication Date: 2024-11-01ZHENGZHOU HOLLOWLITE MATERIALS CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410837717.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The hollow glass microbeads used in new energy vehicles have a high breakage rate during the glue application process, resulting in an increase in the density of the sealant, which cannot achieve lightweighting effect and affects the curing performance of the colloid.

Method used

A divinylbenzene modified polyurethane layer coated with hollow glass microbeads is used to form a polyurethane cladding layer through silane coupling agent activation treatment and polymerization reaction, which improves the compressive strength and elasticity of the microbeads and reduces the breakage rate.

Benefits of technology

The breaking rate of hollow glass microbeads is significantly reduced to less than 5%, the requirements of lightweight sealant are achieved, and the curing performance and construction performance of the colloid are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118879100A_ABST
    Figure CN118879100A_ABST
Patent Text Reader

Abstract

The invention provides an elastic hollow glass bead as well as a preparation method and application thereof. The elastic hollow glass bead is of a core-shell structure and comprises a hollow glass bead located in the core and a divinyl benzene modified polyurethane coating layer arranged on the surface of the hollow glass bead. Wherein the divinyl benzene modified polyurethane coating layer is mainly prepared by carrying out polymerization reaction on isocyanate, polyether polyol and divinyl benzene. As the divinyl benzene modified polyurethane coating layer in the elastic hollow glass bead is made of an elastic material, the divinyl benzene modified polyurethane coating layer coats the surface of the hollow glass bead and has a buffering effect, the hollow glass bead can be well protected from being broken in the gluing process such as potting, the breakage rate is greatly reduced, and the service life of the hollow glass bead is prolonged. According to the present invention, the crushing rate of the hollow glass beads can be reduced to less than 5%, such that the cost can be reduced, and the adhesive colloid can meet the lightweight requirement, has good curing performance, and has good construction performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of materials, and in particular to an elastic hollow glass microsphere and a preparation method and application thereof. Background Art

[0002] New energy vehicles are heavier than traditional energy vehicles. At the same time, based on the current electric vehicle energy supply and energy storage technology, the specific energy of the power batteries currently used in new energy vehicles is much smaller than that of traditional fuel vehicles, which makes the cruising range of new energy vehicles far less than that of traditional fuel vehicles. Therefore, the lightweight technology requirements for new energy vehicles are very urgent. The premise of lightweighting new energy vehicles is to ensure the strength and safety performance of the vehicle, reduce the curb weight of the vehicle as much as possible, thereby improving the power of the vehicle, reducing fuel or electricity consumption, reducing exhaust pollution and increasing driving range.

[0003] New energy vehicle sealants play an irreplaceable role in the all-round protection of batteries. They can prevent electrolyte leakage, resist the influence of the external environment, and improve the reliability of batteries. Therefore, existing sealant manufacturers are committed to the research of lightweight sealants. In order to reduce weight, the introduction of hollow glass microbeads into the sealant can greatly reduce the density of the adhesive, but the introduction of hollow glass microbeads also has certain problems. In order to pursue the maximum low-density sealant, the true density of the hollow glass microbeads used is 0.22-0.28g / cm 3 In this density range, the isostatic compressive strength of hollow glass beads is 5-28MPa, and the breakage rate is about 20%. According to the different colloid viscosities, the pressure of the sealant application process is between 8-20MPa, accompanied by the extrusion rate. The breakage rate of hollow glass beads is very high in this environment. The smaller the true density of hollow glass beads, the higher the breakage rate. For example, the true density is 0.22g / cm 3 The breakage rate of micro-beads is basically over 40%, which leads to two consequences: first, the density of the colloid increases, and the lightweight effect cannot be achieved; second, the hollow glass micro-beads are no longer closed spheres after being broken, and the surface area of ​​the powder is increased after becoming glass fragments, thus affecting the solidification of the colloid.

[0004] Shanghai University of Technology disclosed a hollow glass microsphere coated with phenolic resin and a preparation method thereof in its Chinese invention patent application CN 108822581 A. The hollow glass microspheres in the patent application are of a core-shell structure, wherein the core is the hollow glass microsphere and the shell is the phenolic resin. Although the patent application mentioned that the breakage rate of the hollow glass microspheres coated with phenolic resin in a dynamic grinding environment is low, it did not disclose whether the hollow glass microspheres coated with phenolic resin can be used in automotive sealants to meet the current demand for lightweight automotive sealants. Summary of the invention

[0005] In view of this, it is necessary for the present invention to provide an elastic hollow glass microsphere and a preparation method and application thereof to solve the above problems. One object of the present invention is to provide an elastic hollow glass microsphere and a preparation method thereof, wherein the elastic hollow glass microsphere comprises a polyurethane elastic layer coated on the surface of the hollow glass microsphere, and the polyurethane elastic layer has good elasticity and impact resistance, so that the elastic hollow glass microsphere has a small true density and a high compressive strength.

[0006] Another object of the present invention is to provide an application of the elastic hollow glass microspheres in adhesives, especially in automotive sealants, potting adhesives and structural adhesives. The polyurethane elastic layer of the elastic hollow glass microspheres has a buffering effect, which can better protect the hollow glass microspheres from breaking during the gluing process, greatly reducing the breakage rate, and the breakage rate can be reduced to less than 5%. This not only reduces costs, but also enables the colloid to meet the requirements of lightweight and good curing performance.

[0007] The “breakage rate” in the present invention refers to the volume percentage of the destroyed hollow glass microspheres in the total hollow glass microspheres under a certain isostatic pressure; the “compressive strength” in the present invention, also known as isostatic pressure strength, refers to the breakage rate of the hollow glass microspheres N б The isostatic pressure at that time is expressed in MPa.

[0008] In order to achieve the above object, the technical solution protected by the present invention is as follows:

[0009] An elastic hollow glass microsphere is a core-shell structure, comprising a hollow glass microsphere at the core and a divinylbenzene-modified polyurethane coating layer arranged on the surface of the hollow glass microsphere, and the NCO content of the polyurethane resin in the divinylbenzene-modified polyurethane layer is preferably between 5-8%.

[0010] The NCO content of the divinylbenzene modified polyurethane resin is between 5% and 8%, so that the polyurethane resin has both good elasticity and good hardness. The particle size D90 of the hollow glass microspheres is preferably 65-110 μm, and the true density of the hollow glass microspheres is preferably 0.22-0.28 g / cm 3 , and one of the compressive strengths of 5-28 MPa. The thickness of the divinylbenzene modified polyurethane layer is preferably 0.5-1 μm. The content of divinylbenzene in the divinylbenzene modified polyurethane layer is preferably 4-5%. Wherein, the divinylbenzene modified polyurethane coating layer is mainly prepared by polymerization reaction of isocyanate, polyether polyol and divinylbenzene.

[0011] A method for preparing elastic hollow glass microspheres comprises the following steps:

[0012] Microbead activation: firstly, hollow glass microbeads are activated by using a silane coupling agent to obtain activated microbeads;

[0013] The microspheres are modified, the activated microspheres, isocyanate, polyether polyol and divinylbenzene undergo polymerization reaction, and a divinylbenzene-modified polyurethane coating layer is formed on the surface of the hollow glass microspheres to obtain the elastic hollow glass microspheres; wherein the polyether polyol includes polyether diol and polyether triol, and the NCO content of the polyurethane resin in the divinylbenzene-modified polyurethane layer is between 5-8%.

[0014] The main purpose of the microbead activation step is to increase the interfacial bonding force between the hollow glass microbeads and the divinylbenzene modified polyurethane layer. Therefore, the silane coupling agent can combine with the hydroxyl group, siloxy group, etc. on the surface of the hollow glass microbeads to form a covalent bond, and can combine with the isocyanate group to form a covalent bond. Therefore, the group on the silane coupling agent is preferably at least one of amino, alkyl, thiol, vinyl, epoxy, cyano, and methylvinyloxy groups. The mass of the silane coupling agent is preferably 0.5%-1.5% of the mass of the hollow glass microbeads, such as 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, etc.

[0015] The microbead activation step mainly uses the existing technology to activate the hollow glass microbeads using a silane coupling agent. Specifically, the microbead activation step may include: uniformly mixing the hollow glass microbeads, the silane coupling agent, the first organic solvent and pure water, so that the silane coupling agent reacts chemically with the surface of the hollow glass microbeads to obtain the activated microbeads. More specifically, pure water is first added to the hollow glass microbeads, the first organic solvent and the silane coupling agent, and the addition is completed within 5 minutes, the reaction is carried out for 0.5-1.0 hours, and the activated microbeads are obtained by filtering.

[0016] Among them, the first organic solvent is mainly used to disperse hollow glass microspheres, and the mass ratio of the first organic solvent to the hollow glass microspheres is preferably 1:3.5-4.5, and the first organic solvent is preferably anhydrous ethanol, acetone, or butanone. The main function of the pure water is to hydrolyze the silane coupling agent, so the amount of pure water is preferably 3 times the molar amount of the silane coupling agent, and the conductivity is ﹤10μs / cm. In order to prevent the silane coupling agent from failing, it is best to add it dropwise within 5 minutes. In order to fully activate the microspheres with the silane coupling agent and make the silane coupling agent adhere to the surface of the microspheres as much as possible, the reaction time of the two is preferably 0.5-1.0h.

[0017] The main purpose of the microbead modification step is to form a divinylbenzene-modified polyurethane coating layer on the surface of the activated microbeads, and the coating layer is tightly combined with the hollow glass microbeads. The coating layer is relatively thin and will not significantly change the original density and particle size of the hollow glass microbeads. In the microbead modification process, the activated microbeads, isocyanate and polyether polyol react first to form a polyurethane resin on the surface of the hollow glass microbeads; the polyurethane resin then reacts with divinylbenzene to form a divinylbenzene-modified polyurethane coating layer on the surface of the hollow glass microbeads. Specifically, the microbead modification step may include: first mixing and preheating the activated microbeads, isocyanate and the second solvent, then adding the dehydrated polyether polyol and divinylbenzene to mix, then adding a catalyst, reacting at 65-75°C and vacuum degree -0.095MPa for 1.5-2.0h, cooling and filtering the hollow glass microbeads, and drying at 70-80°C to obtain hollow glass microbeads coated with divinylbenzene-modified polyurethane resin.

[0018] Preferably, in order to promote the reaction between isocyanate and polyether polyol, the preheating temperature of the activated microspheres, isocyanate and the second solvent is 65-75° C. Preferably, the cooling filtration temperature is 40-45° C., which does not affect the filtration of hollow glass microspheres and improves production efficiency.

[0019] In order to ensure that the divinylbenzene modified polyurethane coating layer has good bonding force with the hollow glass microspheres, the mass ratio of the activated microspheres to the divinylbenzene modified polyurethane coating layer is preferably 10:0.85-1.2, and the divinylbenzene modified polyurethane coating layer includes the following raw materials: 1-5 mass parts of isocyanate, 200-300 mass parts of the second solvent, 3-10 mass parts of polyether polyol, 0.01-0.03 mass parts of catalyst and divinylbenzene, and the mass of divinylbenzene is 5% of the total mass of the isocyanate, the second solvent, the polyether polyol and the catalyst, that is, the mass of divinylbenzene is 5% of the total mass of the polyurethane resin in the coating layer, so that the polyurethane resin molecules have a suitable molecular weight to ensure that the polyurethane resin has good elasticity and hardness. Further, in order to avoid or reduce the difference between the NCO% content in the polyurethane resin of the final product and the design value caused by the reaction of water molecules and isocyanate, the polyether polyol added in the microsphere modification step should be dehydrated to remove the water molecules therein.

[0020] The second solvent is preferably xylene, dimethyl carbonate, ethyl acetate or cyclohexane. The isocyanate is preferably a diisocyanate, such as MDI (diphenylmethane diisocyanate), HDI (1,6-hexamethylene diisocyanate), IPDI (isophorone diisocyanate) or TDI (toluene diisocyanate).

[0021] Since polyether diol reacts with isocyanate to generate a linear polymer with good elasticity, and polyether triol reacts with isocyanate to generate a three-dimensional polymer with good strength; therefore, the polymer generated by mixing polyether diol and triol is a mixture of linear and three-dimensional polymers, which has good elasticity and strength, and is beneficial to reducing the breakage rate of hollow glass microspheres during construction; therefore, the polyether polyol includes polyether diol and polyether triol. Preferably, the polyether polyol includes a small molecule polyether triol, a macromolecular polyether triol and a polyether diol, wherein the small molecule polyether triol is used as a cross-linking agent, and its molecular weight is preferably 350-500; the macromolecular polyether triol and the polyether diol are used together as the main body of the polyurethane resin, the molecular weight of the macromolecular polyether triol is preferably 3000-5000, and the molecular weight of the polyether diol is preferably 2000-4000; further, the molar ratio of the small molecule polyether triol, the macromolecular polyether triol and the polyether diol is preferably 1:0.8-2.6:0.9-1.85.

[0022] The catalyst is mainly used to catalyze the reaction of isocyanate, polyether polyol and divinylbenzene, and is preferably at least one of tin and bismuth catalysts, such as dibutyltin dilaurate, dibutyltin dichloride, stannous octoate, dimethyltin dineodecanoate, bismuth neodecanoate and other organic acid tin salts or bismuth salts.

[0023] An application of elastic hollow glass microspheres in an adhesive, the adhesive comprising a main adhesive and elastic hollow glass microspheres. Preferably, the mass percentage of the elastic hollow glass microspheres in the adhesive is 20-30%. The adhesive can be preferably a sealant, a potting adhesive or a structural adhesive, and can be applied to the field of new energy vehicles, such as a sealant for a new energy vehicle battery pack; it can also be applied to other fields.

[0024] The divinylbenzene-modified polyurethane coating layer in the elastic hollow glass microspheres and the elastic hollow glass microspheres prepared by the above method provided by the present invention is tightly bonded to the surface of the hollow glass microspheres and has a relatively thin thickness, such as 0.5-1 μm, which will not significantly change the density and particle size of the original hollow glass microspheres; and the divinylbenzene-modified polyurethane has good elasticity and impact resistance, effectively improving the compressive strength of the elastic hollow glass microspheres.

[0025] When the elastic hollow glass microspheres provided by the present invention are applied to adhesives, since the divinylbenzene-modified polyurethane coating layer in the elastic hollow glass microspheres is made of elastic material and coated on the surface of the hollow glass microspheres, it has a buffering effect and can well protect the hollow glass microspheres from being broken during the gluing process such as potting, thereby greatly reducing the breakage rate, and can reduce the breakage rate of the hollow glass microspheres to less than 5%. This not only reduces costs, but also enables the adhesive colloid to meet the requirements of lightweight and good curing performance, and has good construction performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is a SEM image of the original hollow glass microspheres used in Example 2 of the present invention;

[0027] Figure 2 This is a SEM image of the elastic hollow glass microspheres provided in Example 2 of the present invention. DETAILED DESCRIPTION

[0028] The technical solution of the present invention is further described in detail below through specific implementation methods. The terms used in the present invention are all commonly used terms in the relevant field, and the raw materials, equipment, preparation processes, testing methods, etc. used are all prior arts in the relevant field unless otherwise specified.

[0029] The raw materials used in the following examples and comparative examples include: 3-glycidyloxypropyltrimethoxysilane (Jianghan New Materials, JH-0187), octyltrimethoxysilane (Wuhan Enric, UM08), MDI industrial products (Yantai Wanhua), IPDI industrial products (Bayer), divinylbenzene with a content of 98%, etc.

[0030] The organic reagents used in the embodiments and comparative examples are all industrial products; the pure water used is homemade by a water maker, and the conductivity is less than 10 μs / cm.

[0031] Example 1

[0032] This embodiment provides an elastic hollow glass microsphere, which is a core-shell structure, mainly composed of a hollow glass microsphere located in the core and a divinylbenzene-modified polyurethane coating layer arranged on the surface of the hollow glass microsphere. The raw material formula for its preparation is shown in Table 1.

[0033] This embodiment also provides a method for preparing the elastic hollow glass microspheres, comprising the steps of:

[0034] Microbead activation: hollow glass microbeads, anhydrous ethanol and silane coupling agent were added to a flask according to the formula shown in Table 1, and pure water was added dropwise for 5 minutes. The reaction lasted for 1.0 hours, and the silane-activated microbeads were obtained by filtering.

[0035] Microbead modification: add the activated microbeads, isocyanate and solvent into a flask in proportion, heat to 65°C, add dehydrated polyether polyol and divinylbenzene, add catalyst after mixing, react at 65°C and vacuum degree of -0.095MPa for 1.5h, cool to 45°C, filter out hollow glass microbeads, dry at 70°C to obtain hollow glass microbeads coated with divinylbenzene-modified polyurethane resin.

[0036] Table 1 Formula of elastic hollow glass microspheres provided in Example 1

[0037]

[0038]

[0039] Example 2

[0040] This embodiment provides an elastic hollow glass microsphere, the structure of which is basically the same as that of the elastic hollow glass microsphere provided in Example 1, and the main difference lies in the different raw material formula and preparation process parameters. The raw material formula used in this embodiment is shown in Table 2.

[0041] The method for preparing the elastic hollow glass microspheres provided in this embodiment specifically comprises the following steps:

[0042] Microbead activation: Add the following formula into the flask: Figure 1 The hollow glass microspheres, anhydrous ethanol and silane coupling agent shown in the figure were added with pure water for 5 minutes, reacted for 0.5 hours, and filtered to obtain silane-activated microspheres;

[0043] Microbead modification: Add the activated microbeads, isocyanate and solvent into a flask in proportion, heat to 65°C, add dehydrated polyether polyol and divinylbenzene, mix and add catalyst, react at 70°C, vacuum degree -0.095MPa for 1.5h, cool to 45°C, filter out hollow glass microbeads, dry at 80°C to obtain hollow glass microbeads coated with divinylbenzene-modified polyurethane resin, such as Figure 2 shown.

[0044] Table 2 Formula of elastic hollow glass microspheres provided in Example 2

[0045]

[0046]

[0047] Example 3

[0048] This embodiment provides an elastic hollow glass microsphere, the structure of which is basically the same as that of the elastic hollow glass microsphere provided in Example 1, and the main difference lies in the different raw material formula and preparation process parameters. The raw material formula used in this embodiment is shown in Table 3.

[0049] The method for preparing the elastic hollow glass microspheres provided in this embodiment specifically comprises the following steps:

[0050] Microbead activation: hollow glass microbeads, anhydrous ethanol and coupling agent were added to a flask according to the formula shown in Table 3, and pure water was added dropwise for 5 minutes, reacted for 0.5 hours, and filtered to obtain silane-activated microbeads;

[0051] Microbead modification: add the activated microbeads, isocyanate and solvent into a flask in proportion, heat to 70°C, add dehydrated polyether polyol and divinylbenzene, add catalyst after mixing, react at 70°C and vacuum degree of -0.095MPa for 1.5h, cool to 40°C, filter out hollow glass microbeads, dry at 80°C to obtain hollow glass microbeads coated with divinylbenzene-modified polyurethane resin.

[0052] Table 3 Formula of elastic hollow glass microspheres provided in Example 3

[0053]

[0054]

[0055] Comparative Example

[0056] Comparative Example 1 provides a modified hollow glass microsphere, which is a hollow glass microsphere coated with polyurethane. Its structure and preparation method are basically the same as the elastic hollow glass microsphere provided in Example 2. The main difference is that: divinylbenzene is not added in this comparative example, and the coating layer polyurethane is not modified. The other raw materials and preparation processes are the same.

[0057] Comparative Example 2 provides a modified hollow glass microsphere, which is a hollow glass microsphere coated with polyurethane. Its structure and preparation method are basically the same as the modified hollow glass microspheres provided in Comparative Example 1. The main difference is that: no macromolecular polyether triol and small molecule polyether triol are added in this comparative example, and the other raw materials and preparation processes are the same.

[0058] Comparative Example 3 provides a hollow glass microsphere that has not undergone any modification treatment, and has the same true density and size specifications as the hollow glass microspheres used in Example 2.

[0059] Comparative Example 4 provides a modified hollow glass microsphere, which is a hollow glass microsphere coated with polyurethane. Its structure and preparation method are basically the same as the elastic hollow glass microsphere provided in Example 3. The main difference is that: divinylbenzene is not added in this comparative example, and the coating layer polyurethane is not modified. The other raw materials and preparation processes are the same.

[0060] Comparative Example 5 provides a modified hollow glass microsphere, which is a hollow glass microsphere coated with polyurethane. Its structure and preparation method are basically the same as the modified hollow glass microspheres provided in Comparative Example 4. The main difference is that no polyether diol is added in this comparative example, and the other raw materials and preparation processes are the same.

[0061] Comparative Example 6 provides a hollow glass microsphere that has not undergone any modification treatment, and has the same true density and size specifications as the hollow glass microsphere used in Example 3.

[0062] Application Examples

[0063] This embodiment provides an application of elastic hollow glass microspheres in adhesives. Specifically, the elastic hollow glass microspheres and silicone resin (component A is vinyl silicone oil, component B is hydrogenated silicone oil and catalyst) are placed in a homogenizer at a mass ratio of 32:112 and mixed for 5 minutes to prepare a lightweight silicone resin glue. The elastic hollow glass microspheres are the elastic hollow glass microspheres provided in any one of embodiments 1-3.

[0064] Performance Verification

[0065] Samples: elastic hollow glass microspheres provided in Examples 1-3, modified hollow glass microspheres provided in Comparative Examples 1-2 and 4-5, unmodified hollow glass microspheres provided in Comparative Examples 3 and 6, and lightweight silicone resin glue provided in the application examples using the hollow glass microspheres provided in Examples 1-3 and Comparative Examples 1-6, respectively.

[0066] The above samples were tested for compressive strength, breakage rate during construction of lightweight silicone resin glue at 15MPa and 25MPa glue pressures, and cured appearance. The results are shown in Table 4.

[0067] 1. Curing time test: The curing time of the hollow glass microspheres provided in Examples 1-3 and Comparative Examples 1-5 at the colloid application pressure of 15 MPa and 25 MPa was tested respectively with reference to the current national standards.

[0068] 2. Breakage rate test: 1) Use a 50CC density cylinder to test the initial density of lightweight silicone resin glue and record the data; 2) Pressurize the glue in the quantitative cylinder; 3) Pressurize about 20CC each time, and each pressure is completed in 3 times; 4) After each pressurization, slow dynamic movement for 5 minutes to ensure uniform force; 5) After the pressurization is completed, use a 50CC density cylinder to test and record the density data; 6) According to the density data before and after pressurization, the breakage rate of hollow glass beads is calculated by an empirical formula; Among them, the pressure applied to the glue is 15MPa and 25MPa respectively.

[0069] Table 4 Performance test results

[0070]

[0071]

[0072] Combined with Table 4, from the comparative data of Example 2 and Comparative Examples 1-3, and the comparative data of Example 3 and Comparative Examples 4-6, it can be seen that the elastic hollow glass microspheres provided in the embodiment of the present invention are divinylbenzene-modified polyurethane coating layers formed on the surface of the existing hollow glass microspheres, so that the elastic hollow glass microspheres not only have high strength, but also have high elasticity. Therefore, when the above-mentioned elastic hollow glass microspheres are applied to the adhesive, the hollow glass microspheres can be better protected from being broken during the gluing process such as potting, and the breakage rate is greatly reduced. The breakage rate of the hollow glass microspheres can be lower than 5%, which can not only reduce the cost, but also shorten the curing time of the adhesive colloid while meeting the lightweight requirements, improve the construction efficiency, and have good construction performance.

[0073] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, ordinary technicians in the field should understand that the specific implementation methods of the present invention can still be modified or some technical features can be replaced by equivalents without departing from the spirit of the technical solution of the present invention, which should be included in the scope of the technical solution for protection of the present invention.

Claims

1. An elastic hollow glass microsphere, characterized in that: A core-shell structure, comprising hollow glass microspheres at the core and a divinylbenzene-modified polyurethane coating layer disposed on the surface of the hollow glass microspheres, wherein the NCO content of the polyurethane resin in the divinylbenzene-modified polyurethane layer is between 5% and 8%; Preferably, the content of divinylbenzene in the divinylbenzene-modified polyurethane layer is 4-5%; Preferably, the particle size D90 of the hollow glass microspheres is 65-110 μm, and the true density of the hollow glass microspheres is preferably 0.22-0.28 g / cm 3 , and one of the compressive strengths of 5-28 MPa; Preferably, the divinylbenzene-modified polyurethane coating layer is mainly prepared by polymerization reaction of isocyanate, polyether polyol and divinylbenzene, wherein the polyether polyol includes polyether diol and polyether triol.

2. The elastic hollow glass microsphere according to claim 1, characterized in that: The thickness of the divinylbenzene modified polyurethane layer is 0.5-1 μm.

3. A method for preparing the elastic hollow glass microspheres according to claim 1 or 2, comprising the steps of: Microbead activation: firstly, hollow glass microbeads are activated by using a silane coupling agent to obtain activated microbeads; Microsphere modification, the activated microspheres, isocyanate, polyether polyol and divinylbenzene undergo polymerization reaction, and a divinylbenzene-modified polyurethane coating layer is formed on the surface of the hollow glass microspheres to obtain the elastic hollow glass microspheres; wherein, The polyether polyol includes polyether diol and polyether triol, and the NCO content of the polyurethane resin in the divinylbenzene modified polyurethane layer is between 5% and 8%; Preferably, the mass ratio of the activated microbeads to the divinylbenzene-modified polyurethane coating layer is 10:0.85-1.

2.

4. The preparation method according to claim 3, characterized in that: The divinylbenzene-modified polyurethane coating layer comprises the following raw materials: 1 to 5 parts by mass of isocyanate, 200 to 300 parts by mass of a second solvent, 3 to 10 parts by mass of a polyether polyol, 0.01 to 0.03 parts by mass of a catalyst and divinylbenzene, wherein the mass of the divinylbenzene is 5% of the total mass of the isocyanate, the second solvent, the polyether polyol and the catalyst; Preferably, the polyether polyol comprises a small molecule polyether triol, a macromolecular polyether triol and a polyether diol, wherein the molecular weight of the small molecule polyether triol is 350-500, the molecular weight of the macromolecular polyether triol is 3000-5000, and the molecular weight of the polyether diol is 2000-4000; Preferably, the molar ratio of the small molecule polyether triol, the macromolecular polyether triol and the polyether diol is 1:0.8-2.6:0.9-1.

85.

5. The preparation method according to claim 4, characterized in that: The microbead modification step comprises: firstly mixing the activated microbeads, isocyanate and a second solvent and preheating them, then adding a dehydrated polyether polyol and divinylbenzene to mix, then adding a catalyst, reacting at 65-75° C. and a vacuum degree of -0.095 MPa for 1.5-2.0 h, cooling and filtering out the hollow glass microbeads, and drying at 70-80° C. to obtain hollow glass microbeads coated with divinylbenzene-modified polyurethane resin; Preferably, the mixed preheating temperature of the activated microbeads, isocyanate and the second solvent is 65-75°C; Preferably, the temperature of the cooling and filtering treatment is 40-45°C.

6. The preparation method according to any one of claims 3 to 5, characterized in that: The groups on the silane coupling agent include at least one of amino, alkyl, mercapto, vinyl, epoxy, cyano and methylvinyloxy groups; Preferably, the mass of the silane coupling agent is 0.5%-1.5% of the mass of the hollow glass microspheres.

7. The preparation method according to claim 6, characterized in that: The microbead activation step comprises: uniformly mixing the hollow glass microbeads, a silane coupling agent, a first organic solvent and pure water, so that the silane coupling agent reacts chemically with the surface of the hollow glass microbeads to obtain the activated microbeads; Preferably, the mass ratio of the first organic solvent to the hollow glass microspheres is 1: 3.5-4.5; Preferably, the first organic solvent is one or any combination of anhydrous ethanol, acetone or butanone; Preferably, the amount of pure water is 3 times the molar amount of the silane coupling agent.

8. The preparation method according to claim 7, characterized in that: The microbead activation step includes: firstly adding pure water to the hollow glass microbeads, the first organic solvent and the silane coupling agent, and the dropping is completed within 5 minutes, reacting for 0.5-1.0 hours, filtering, and obtaining the activated microbeads.

9. The preparation method according to claim 4, characterized in that: The second solvent is xylene, dimethyl carbonate, ethyl acetate or cyclohexane, the isocyanate is diisocyanate; the catalyst is organic acid tin salt or bismuth salt such as dibutyltin dilaurate, dibutyltin dichloride, stannous octoate, dimethyltin dineodecanoate, bismuth neodecanoate, etc.

10. Application of elastic hollow glass microspheres in adhesives; Preferably, the mass percentage of the elastic hollow glass microspheres in the adhesive is 20-30%; Preferably, the adhesive is a sealant, a potting adhesive or a structural adhesive; Preferably, the adhesive is used in the field of new energy vehicles.

Citation Information

Cited By

  • Waste carpet recycled PA hollow glass bead composite material and preparation method thereof