Preparation method of modified alumina slurry with high solid content and low viscosity
By forming a polymer interface layer on the surface of alumina particles, the problems of high content uniform dispersion and low viscosity slurry preparation at room temperature are solved, and the preparation of high solid content and low viscosity alumina slurry is achieved, avoiding the High temperature treatment and improve the fluidity of the slurry.
Patent Information
- Application Number
- CN202411345763.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-26
- Publication Date
- 2024-11-01
AI Technical Summary
The existing preparation methods of alumina slurry require high temperature treatment and rely on organic matter containing Si-O segments, making it difficult to achieve high content uniform dispersion of alumina particles and low viscosity slurry preparation at room temperature.
By preparing organoaluminum sol and modified alumina particles, adjust the pH value to 7-9 using tris solution, add catecholamines and react with alumina particles at room temperature to form a polymer interface layer, and achieve surface modification of alumina particles. , and the modified alumina particles were stirred and dispersed in the organoaluminum solution to prepare a high solids content and low viscosity alumina slurry.
The preparation of alumina slurry of up to 30%-50% solid content and low viscosity (30-500 mpa·s) is achieved, avoiding high temperature treatment and improving particle spacing and fluidity.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of alumina slurry, and in particular to a method for preparing a modified alumina slurry with high solid content and low viscosity. Background Art
[0002] Alumina has excellent mechanical, thermal and optical properties and is widely used in engineering ceramics, gemstone industry and solid electrolytes. Dispersing alumina in a solvent to form a slurry with a specific viscosity is one of the simplest methods for preparing alumina coatings. In order to increase the solid content of alumina in the slurry, the surface of alumina powder is generally modified. Currently, the commonly used surface modification method is mainly the wet process. Patent CN202211563985.X shows a method of utilizing lanthanum phosphate solution, by adding high-purity nano-alumina powder to the lanthanum phosphate precursor solution and mixing them evenly in a high-speed disperser, then heating the mixture to obtain a gel mixed system, and finally performing high-temperature sintering to obtain a solid, adding deionized water and ball milling to obtain a high-solid content, low-viscosity alumina slurry; Patent CN202211566008.5 shows a method for modifying a silane coupling agent, by adjusting the pH value of the aqueous solution to form a stable silane coupling agent monomolecular hydrolyzate, dispersing alumina therein, then using protective gas blowing to remove water, and performing wet modification under reduced pressure conditions, and finally forming a slurry by adding methyl-terminated polydimethylsiloxane.
[0003] The above methods all require high temperature treatment of alumina particles to achieve surface modification. On the other hand, the formation of alumina slurry always depends on organic matter containing Si-O segments, which is not only difficult to remove, but also forms SiO2 at high temperatures. Therefore, it is urgent to develop a method that can achieve surface modification of alumina particles at room temperature, so that alumina particles can be evenly dispersed in a solvent at a higher content. Summary of the invention
[0004] The object of the present invention is to provide a method for preparing a modified alumina slurry with high solid content and low viscosity, so as to solve the problems raised in the above background technology.
[0005] In order to achieve the above object, the present invention adopts the following technical scheme: a method for preparing a modified alumina slurry with high solid content and low viscosity, comprising the following steps: 1) preparing an organic aluminum sol: dissolving an organic aluminum salt in a solvent to obtain an organic aluminum sol for later use; 2) Preparation of modified alumina particles: taking a tris solution and adjusting the pH value to 7-9, then adding catecholamine substances to obtain a catecholamine solution, adding alumina particles to the catecholamine solution, and then stirring the reaction at room temperature, and filtering to obtain modified alumina particles; 3) The organic aluminum sol in step 1 is mixed with ionized water to obtain an organic aluminum solution, and the obtained modified aluminum oxide particles are stirred and dispersed in the organic aluminum solution, stirred and mixed, and modified aluminum oxide slurry is obtained after sufficient reaction.
[0006] Compared with the existing technology, this solution prepares a polymer interface layer on the surface of alumina particles, modifies the particle surface, increases the distance between alumina particles, effectively improves the agglomeration effect between alumina particles, and achieves the preparation of slurry with a solid content of up to 30%-50%, and the viscosity value is only 30-500 mpa·s. At the same time, this solution provides a wet modification without high-temperature treatment, realizing the surface modification of alumina particles at room temperature.
[0007] The reaction mechanism is as follows: the pH value of the system is adjusted to 7-9 using a tris (trishydroxymethylaminomethane) solution. This step is intended to create an environment that is conducive to the reaction of catecholamines with the surface of alumina particles. Catecholamines (such as dopamine, norepinephrine, etc.) show stronger reactivity under alkaline conditions. Secondly, catecholamines interact with the hydroxyl (-OH) on the surface of alumina particles under alkaline conditions and adsorb on the surface of the particles through hydrogen bonds, coordination bonds or covalent bonds. This adsorption not only changes the chemical properties of the particle surface, but also forms a polymer interface layer between the particles, thereby increasing the distance between the particles. The surface of the modified alumina particles has a polymer interface layer, which plays a "lubricating" role in the slurry, reducing direct contact and agglomeration between particles. At the same time, the presence of the polymer interface layer also increases the distance between particles, further improving the fluidity and viscosity of the slurry.
[0008] Preferably, the organic aluminum salt in the above step 1 is one or both of aluminum isopropoxide and aluminum sec-butoxide, and the solvent is any one of water, alcohol and acetone.
[0009] Preferably, the catecholamine substances in the above step 2 are one or more of levodopa, dopamine, norepinephrine and epinephrine.
[0010] Specifically, in the above step 2, the amount of the catecholamine substance added is 1-40 mg / mL based on the tris solution, the diameter of the aluminum oxide particles ranges from nanometers to micrometers, and the amount of the aluminum oxide particles added is less than 0.5 g / mL.
[0011] Preferably, in the above step 2, the stirring speed is 100-1000 rpm and the reaction time is 6-48 h.
[0012] In order to achieve better technical effects, a further technical solution also includes: the modified alumina particles obtained after filtration are washed with alcohol, acetone or water.
[0013] Preferably, the mass fraction of the modified alumina particles added in the above step 3 is less than 50%.
[0014] Specifically, in the above step 3, the stirring speed is 400 rpm to 3000 rpm, and the reaction time is 1-12 h.
[0015] In order to achieve better technical effects, further technical measures also include: adding ceramic particles to the modified alumina slurry obtained in the above step 3.
[0016] Adding additional ceramic particles to the resulting alumina slurry can achieve modification of coating properties, reflecting the scalability potential of the above-mentioned alumina slurry.
[0017] Preferably, the ceramic particles are one or more of SiO2 ceramic particles, mica ceramic particles, and yttrium oxide ceramic particles, with a mass fraction of less than 2%.
[0018] Compared with the prior art, the present invention has the following beneficial effects: the present solution prepares a polymer interface layer on the surface of alumina particles, modifies the particle surface, increases the spacing between alumina particles, effectively improves the agglomeration effect between alumina particles, realizes the preparation of slurry with a solid content of up to 30%-50%, and the viscosity value is only 30-500 mpa·s. At the same time, the present solution provides a wet modification without high temperature treatment, realizing the surface modification of alumina particles at room temperature. DETAILED DESCRIPTION
[0019] The following description is used to disclose the present invention so that those skilled in the art can implement the present invention. The preferred embodiments described below are only examples, and those skilled in the art can think of other obvious variations. The basic principles of the present invention defined in the following description can be used for other embodiments, variations, improvements, equivalents, and other technical solutions that do not deviate from the spirit and scope of the present invention.
[0020] A method for preparing a high-solid content and low-viscosity modified alumina slurry comprises the following steps: 1) preparing an organic aluminum sol: dissolving an organic aluminum salt in a solvent to obtain an organic aluminum sol, wherein the organic aluminum salt is one or both of aluminum isopropoxide and aluminum sec-butoxide, and the solvent is any one of water, alcohol, and acetone for later use; 2) Prepare modified alumina particles: take tris solution and adjust the pH value to 7-9, then add catecholamines to obtain a catecholamine solution, add alumina particles to the catecholamine solution, and then stir the reaction at room temperature. The stirring speed is 100-1000rpm, and the reaction time is 6-48h. The modified alumina particles obtained after filtering are washed with alcohol, acetone or water. The catecholamines are one or more of levodopa, dopamine, norepinephrine and epinephrine. The amount of catecholamines added is 1-40mg / mL based on tris solution. The diameter of the alumina particles ranges from nanometers to micrometers. The amount of alumina particles added is less than 0.5g / mL. 3) The organic aluminum sol in step 1 is mixed with ionized water to obtain an organic aluminum solution, and the modified aluminum oxide particles obtained are stirred and dispersed in the organic aluminum solution. The mass fraction of the modified aluminum oxide particles added is less than 50%, and the mixture is stirred and mixed at a stirring speed of 400 rpm to 3000 rpm. The reaction time is 1 to 12 hours. After sufficient reaction, the modified aluminum oxide slurry is obtained.
[0021] In order to achieve better technical effects, ceramic particles are added to the modified alumina slurry obtained in the above step 3. The ceramic particles are one or more of SiO2 ceramic particles, mica ceramic particles, and yttrium oxide ceramic particles, with a mass fraction of less than 2%.
[0022] The present invention is further described in detail below with reference to the embodiments. Example 1
[0023] 1 mol of aluminum isopropoxide was dispersed in 500 mL of water to obtain an organic aluminum sol having a solid content of 5% and a viscosity of 10 mPa·s.
[0024] Take 10 mL of tris solution, adjust the pH value to 8.5, add 20 mg / mL of levodopa to obtain a levodopa solution, add 5 g of alumina particles, and react at a speed of 200 rpm for 24 hours to obtain modified alumina particles.
[0025] The obtained modified alumina was dissolved in 10 mL of organic aluminum sol and stirred for dispersion at a stirring speed of 1000 rpm for 2 h. The obtained alumina slurry had a solid content of 45% and a viscosity of 350 mpa·s. Example 2
[0026] Preparation of organic aluminum sol: 0.3 mol of aluminum sec-butoxide was dissolved in 300 mL of acetone to obtain an organic aluminum sol with a solid content of 3% and a viscosity of about 5 mPa·s.
[0027] Preparation of modified alumina particles: 5 mL of tris solution was taken, the pH value was adjusted to 7, dopamine was added to a concentration of 1 mg / mL, and then 0.1 g of nano-alumina particles was added, and the reaction was stirred at 100 rpm for 48 h, filtered and washed with acetone.
[0028] Mixing to prepare slurry: The modified alumina particles were dispersed in 5 mL of organic aluminum sol at a mass fraction of 10%, with a stirring speed of 400 rpm and a stirring time of 1 h to obtain a modified alumina slurry with a solid content of 3% and a viscosity of about 30 mPa·s. Example 3
[0029] Preparation of organic aluminum sol: 2 mol of aluminum isopropoxide was dissolved in 1000 mL of alcohol to obtain an organic aluminum sol with a solid content of 10% and a viscosity of about 20 mPa·s.
[0030] Preparation of modified alumina particles: Take 20 mL of tris solution, adjust the pH to 9, add norepinephrine to a concentration of 40 mg / mL, then add 10 g of micron-sized alumina particles, stir at 1000 rpm for 6 h, filter and wash with alcohol.
[0031] Mixing to prepare slurry: The modified alumina particles were dispersed in 20 mL of organic aluminum sol at a mass fraction of 48%, with a stirring speed of 3000 rpm and a stirring time of 12 h to obtain a modified alumina slurry with a solid content of 48% and a viscosity of about 500 mPa·s. Example 4
[0032] Preparation of organic aluminum sol: 1 mol of aluminum isopropoxide and 0.5 mol of aluminum sec-butoxide were mixed and dissolved in 800 mL of water to obtain an organic aluminum sol with a solid content of 7.5% and a viscosity of about 15 mPa·s.
[0033] Preparation of modified alumina particles: Take 15 mL of tris solution, adjust the pH to 8, add epinephrine to a concentration of 25 mg / mL, then add 3 g of nano- to micro-mixed alumina particles, stir the reaction at 500 rpm for 12 h, filter and wash with deionized water.
[0034] Mixing to prepare slurry: The modified alumina particles were dispersed in 15 mL of organic aluminum sol at a mass fraction of 30%, with a stirring speed of 1500 rpm and a stirring time of 6 h to obtain a modified alumina slurry with a solid content of 22.5% and a viscosity of about 250 mPa·s. Example 5
[0035] Preparation of organic aluminum sol: 0.1 mol of aluminum isopropoxide was dissolved in 50 mL of water to obtain an organic aluminum sol with a solid content of 2% and a viscosity of about 3 mPa·s.
[0036] Preparation of modified alumina particles: 2 mL of tris solution was taken, the pH value was adjusted to 7.5, levodopa was added to a concentration of 5 mg / mL, and then 0.05 g of nano-alumina particles was added, and the reaction was stirred at 200 rpm for 12 h, filtered and washed with deionized water.
[0037] Mixing to prepare slurry: The modified alumina particles were dispersed in 2 mL of organic aluminum sol at a mass fraction of 10%, with a stirring speed of 800 rpm and a stirring time of 4 h to obtain a modified alumina slurry with a solid content of 2% and a viscosity of about 30 mPa·s. Example 6
[0038] Preparation of organoaluminum sol: 2.5 mol of aluminum sec-butoxide was dissolved in 1250 mL of alcohol to obtain an organoaluminum sol with a solid content of 12.5% and a viscosity of about 25 mPa·s.
[0039] Preparation of modified alumina particles: Take 30 mL of tris solution, adjust the pH to 8.8, add a mixture of dopamine and norepinephrine to a total concentration of 35 mg / mL (half each), then add 12 g of micron-sized alumina particles, stir at 800 rpm for 8 h, filter and wash with acetone.
[0040] Mixing to prepare slurry: The modified alumina particles were dispersed in 30 mL of organoaluminum sol at a mass fraction of 49%, with a stirring speed of 2500 rpm and a stirring time of 8 h to obtain a modified alumina slurry with a solid content of 61.25% (considering the solid content of the organoaluminum sol itself), but marked as close to 50%, and a viscosity of about 450 mPa·s. Example 7
[0041] The modified alumina slurry was prepared according to the method of Example 4.
[0042] Add ceramic particles: Add SiO2 ceramic particles to the modified alumina slurry with a mass fraction of 1%. Stir and mix thoroughly to ensure that the ceramic particles are evenly dispersed in the slurry. Example 8
[0043] The modified alumina slurry was prepared according to the method of Example 4.
[0044] Add ceramic particles: Add mica ceramic particles to the obtained modified alumina slurry with a mass fraction of 1.5%. Stir and mix thoroughly. Example 9
[0045] The modified alumina slurry was prepared according to the method of Example 4.
[0046] Add ceramic particles: Add yttrium oxide ceramic particles to the obtained modified alumina slurry with a mass fraction of 0.8%. Stir and mix thoroughly. Example 10
[0047] The modified alumina slurry was prepared according to the method of Example 4.
[0048] Add ceramic particles: Add SiO2 ceramic particles, mica ceramic particles and yttrium oxide ceramic particles to the modified alumina slurry at the same time, with a total mass fraction of 2%. Stir and mix thoroughly to ensure that the three ceramic particles are evenly dispersed in the slurry.
[0049] Those skilled in the art should understand that the embodiments of the present invention shown in the above description are only examples and do not limit the present invention. The purpose of the present invention has been fully and effectively achieved. The functions and structural principles of the present invention have been demonstrated and explained in the embodiments, and the embodiments of the present invention may be deformed or modified in any way without departing from the principles.
Claims
1. A method for preparing a high solid content and low viscosity modified alumina slurry, characterized in that The following steps are involved: 1) preparing an organic aluminum sol: dissolving an organic aluminum salt in a solvent to obtain an organic aluminum sol for later use; 2) Preparation of modified alumina particles: taking a tris solution and adjusting the pH value to 7-9, then adding catecholamine substances to obtain a catecholamine solution, adding alumina particles to the catecholamine solution, and then stirring the reaction at room temperature, and filtering to obtain modified alumina particles; 3) The organic aluminum sol in step 1 is mixed with ionized water to obtain an organic aluminum solution, and the obtained modified aluminum oxide particles are stirred and dispersed in the organic aluminum solution, stirred and mixed, and modified aluminum oxide slurry is obtained after sufficient reaction.
2. The method for preparing a high solid content and low viscosity modified alumina slurry according to claim 1, characterized in that: The organic aluminum salt in step 1 is one or both of aluminum isopropoxide and aluminum sec-butoxide, and the solvent is any one of water, alcohol, and acetone.
3. The method for preparing a high solid content and low viscosity modified alumina slurry according to claim 2, characterized in that: The catecholamine substances in step 2 are one or more of levodopa, dopamine, norepinephrine and epinephrine.
4. The method for preparing a high solid content and low viscosity modified alumina slurry according to claim 3, characterized in that: In step 2, the amount of catecholamines added is 1-40 mg / mL based on tris solution, the diameter of the aluminum oxide particles ranges from nanometer to micrometer, and the amount of aluminum oxide particles added is less than 0.5 g / mL.
5. The method for preparing a high solid content and low viscosity modified alumina slurry according to claim 4, characterized in that: In the step 2, the stirring speed is 100-1000 rpm and the reaction time is 6-48 h.
6. The method for preparing a high solid content and low viscosity modified alumina slurry according to claim 5, characterized in that: The modified alumina particles obtained after filtration are washed with alcohol, acetone or water.
7. The method for preparing a high solid content and low viscosity modified alumina slurry according to claim 6, characterized in that: The mass fraction of the modified alumina particles in step 3 is less than 50%.
8. The method for preparing a high solid content and low viscosity modified alumina slurry according to claim 7, characterized in that: In the step 3, the stirring speed is 400 rpm to 3000 rpm, and the reaction time is 1 to 12 hours.
9. The method for preparing a modified alumina slurry with high solid content and low viscosity according to any one of claims 1 to 8, characterized in that: Ceramic particles are added to the modified alumina slurry obtained in step 3.
10. The method for preparing a high solid content and low viscosity modified alumina slurry according to claim 9, characterized in that: The ceramic particles are one or more of SiO2 ceramic particles, mica ceramic particles, and yttrium oxide ceramic particles, with a mass fraction of less than 2%.
Citation Information
Patent Citations
Dopamine compound modified or coated nano particle modified polymer composite material and preparation method thereof
CN105440583A
Aluminum oxide waterproof coating for nitrogen-oxygen sensor and preparation method of aluminum oxide waterproof coating
CN117986900A
Slurry composition
KR101483451B1
Nanoporous ultrafine alpha-alumina powders and freeze drying process of preparing same
US20040198584A1
Aluminas and methods for producing same
WO2020072607A1