Forming method and application of hollow spherical composite lithium adsorption material

By modifying the in-situ function of powder lithium ion sieve and induced phase conversion method of solvent volatility, hollow spherical composite lithium adsorption materials were prepared, solving the problems of lithium adsorption capacity and structural stability in the prior art, and achieving efficient lithium ion adsorption and simplified forming process, suitable for industrialization of sea brine lithium extraction.

CN118904279AActive Publication Date: 2024-11-08TIANJIN UNIV OF SCI & TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410969547.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08
Estimated Expiration
2044-07-19

AI Technical Summary

Technical Problem

In actual application, the existing composite lithium adsorption materials have reduced the lithium adsorption capacity and adsorption rate due to the polymer material shielding the active adsorption site, poor interfacial compatibility and structural stability, and cumbersome molding steps, making it difficult to achieve large-scale production.

Method used

By modifying the in-situ function of the powder lithium ion sieve and using the solvent volatilization-induced phase conversion method, hollow spherical composite lithium adsorption material is prepared, and ultrasonic dispersion and cast film liquid phase conversion technology is used to form a hollow spherical structure to improve the lithium ion sieve Adsorption capacity and structural stability.

Benefits of technology

It has achieved the improvement of lithium adsorption capacity and structural stability, and maintained an adsorption capacity of more than 90% in actual applications. It is suitable for the industrialization of sea brine lithium extraction, simplified the molding process, and is suitable for lithium such as titanium, manganese, aluminum, etc. Preparation of ion sieve.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904279A_ABST
    Figure CN118904279A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of preparation of composite lithium adsorption materials, and relates to a forming method and application of a hollow spherical composite lithium adsorption material, and the preparation method comprises the following steps: adding a powder lithium ion sieve and a catecholamine compound into a low-boiling-point solvent, and dispersing to obtain a suspension; adding polysulfone into the suspension, and stirring at room temperature to prepare a membrane casting solution; the prepared membrane casting solution is sucked into a needle tube, a water and ethanol cosolvent is used as a receiving solution, the volume of ethanol in the receiving solution is 0-20%, the membrane casting solution is dropwise added at the position 10-20 cm above the liquid level of the receiving solution, after phase inversion, pure water is used for full washing, and the hollow spherical composite lithium adsorption material is obtained. The forming method is simple and easy to implement, and the prepared hollow spherical composite lithium adsorption material is high in lithium adsorption capacity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of preparation of composite lithium adsorption materials, and in particular relates to a molding method and application of a hollow spherical composite lithium adsorption material. Background Art

[0002] As an important element supporting the country's new energy strategy, lithium is recognized as a "green energy metal" and "white oil" that promotes world progress. It is widely used in new energy vehicles, aerospace and other fields. Seawater, geothermal water and salt lake brine contain more than 60% of the earth's total lithium resources. The efficient development of lithium resources in seawater, underground brine and salt lake brine has important economic value and strategic significance.

[0003] The adsorption method is currently recognized as the most promising method for extracting lithium from sea brine. Its core technology is to use the inorganic lithium ion sieve (LIS) adsorbent structure to + The "memory effect" of Li + Separation and enrichment. However, LIS usually exists in the form of powder, and its industrial application is limited by problems such as easy agglomeration, easy loss, and difficult recovery. In order to solve these industrial problems, composite lithium adsorption materials in the form of granules, foams, sponges, flat films, and fibers have been prepared through molding techniques such as immersion phase inversion, freeze drying, and electrospinning.

[0004] However, these composite lithium adsorption materials have three new problems in practical application: first, due to the "shielding effect" of polymer materials on the active adsorption sites of LIS, their lithium adsorption capacity and adsorption rate are both reduced; second, due to the lack of interaction between inorganic LIS and organic polymers, their interface compatibility and structural stability are poor; third, the molding steps reported so far are relatively cumbersome and difficult to achieve large-scale production. These problems further limit the practical application of current composite lithium adsorption materials. Summary of the invention

[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a method for forming a hollow spherical composite lithium adsorption material and its application. By in-situ functional modification of a powdered lithium ion sieve and a solvent evaporation-induced phase transformation method, a hollow spherical composite lithium adsorption material with high lithium adsorption capacity is obtained.

[0006] The technical solution adopted by the present invention to solve the technical problem is:

[0007] On one hand, the present invention provides a method for forming a hollow spherical composite lithium adsorption material, which is prepared by inducing phase transformation by solvent volatilization. The specific operation is:

[0008] (1) adding 1.0-6.0 wt% of lithium ion sieve powder and 0.05-0.2 wt% of catecholamine compounds to a low boiling point solvent, dispersing the lithium ion sieve powder under 400-600 W ultrasound for 20-40 minutes to obtain a suspension;

[0009] (2) adding 2.0-6.0 wt % of polysulfone to the suspension, stirring for 2-5 h at room temperature of 20-25° C., to prepare a casting solution;

[0010] (3) The casting solution prepared in step (2) is sucked into a syringe, and water + ethanol co-solvent is used as a receiving solution, the volume of ethanol in the receiving solution is 0-20%, and the casting solution is dripped dropwise at a height of 10-20 cm above the liquid surface of the receiving solution, and after 1-2 hours of phase conversion, it is fully washed with pure water to obtain a hollow spherical composite lithium adsorbent material. Among them, adding an appropriate proportion of ethanol from water helps to reduce the surface tension of the receiving solution, thereby regulating the spherical wall thickness and microporous structure of the hollow spherical composite lithium adsorbent material, but when the ethanol content exceeds 20%, the spherical wall thickness is too small and becomes a deflated sheet.

[0011] Furthermore, the powder lithium ion sieve is a titanium lithium ion sieve, a manganese lithium ion sieve, an aluminum lithium ion sieve, etc.

[0012] Furthermore, the casting solution contains 3.0-5.0 wt% polysulfone.

[0013] Furthermore, the volume of ethanol in the receiving solution is 0 to 10.0%.

[0014] Furthermore, the role of the catecholamine compound is to achieve hydrophilic functional modification of the powder ion sieve through oxidation-self-polymerization, and the catecholamine compound is one or more of dopamine hydrochloride, catechol, tannic acid, gallic acid, and meta-phenylenediamine.

[0015] Furthermore, the low boiling point solvent is one or more of dichloromethane, carbon disulfide, chloroform and tetrahydrofuran.

[0016] Furthermore, the polysulfone serves as a carrier for coating the powdered lithium ion sieve. The polysulfone may also be polyvinyl chloride or polyvinylidene fluoride.

[0017] Another aspect of the present invention provides an application of the hollow spherical composite lithium adsorption material prepared by the molding method in adsorbing lithium.

[0018] Furthermore, the hollow spherical composite lithium adsorption material is dispersed in a lithium-containing solution with a pH of 11.5 to 12.5 at a solid-liquid ratio of 1:100 to 1:200, and the adsorption capacity is tested using an inductively coupled plasma emission spectrometer.

[0019] The advantages and positive effects of the present invention are:

[0020] (1) The present invention utilizes green bionic materials to achieve in-situ functional modification of powdered ion sieves during the molding process, and obtains a composite lithium adsorption material in the form of a hollow sphere by a solvent evaporation-induced phase transformation method. The molding method is simple and easy, and the lithium ion sieve in the prepared hollow spherical composite lithium adsorption material tends to be enriched on the inner and outer surfaces of the hollow sphere, showing a lithium adsorption capacity equivalent to that of the powdered lithium ion sieve. Moreover, after being applied to actual underground brine for 5 cycles, the adsorption capacity can still be maintained at more than 90%, showing good cycle stability;

[0021] (2) This molding technology is universal and can be applied to titanium, manganese, aluminum and other powder lithium ion sieves. It can even be further expanded to be suitable for the molding and preparation of composite adsorption materials for adsorbing bromine, rubidium, cesium and strontium ions. It can provide a technical support for the industrialization of lithium extraction from sea brine and has great prospects for industrial application. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a physical picture of the hollow spherical composite lithium adsorption material prepared in Example 1 of the present invention;

[0023] Figure 2 This is a particle size distribution diagram of the hollow spherical composite lithium adsorption material prepared in Example 1 of the present invention;

[0024] Figure 3 This is a graph showing the lithium adsorption performance of the hollow spherical composite lithium adsorption material prepared in Example 1 of the present invention;

[0025] Figure 4 This is a physical picture of the hollow spherical composite lithium adsorption material prepared in Example 2 of the present invention;

[0026] Figure 5 This is a graph showing the lithium adsorption performance of the hollow spherical composite lithium adsorption material prepared in Example 2 of the present invention;

[0027] Figure 6 This is a graph showing the lithium adsorption performance of the hollow spherical composite lithium adsorption material prepared in Example 3 of the present invention;

[0028] Figure 7 This is a graph showing the lithium adsorption performance of the hollow spherical composite lithium adsorption material prepared in Comparative Example 1;

[0029] Figure 8 This is a physical picture of the hollow spherical composite lithium adsorption material prepared in Comparative Example 2;

[0030] Fig. 9 This is a graph showing the lithium adsorption performance of the hollow spherical composite lithium adsorption material prepared in Comparative Example 2;

[0031] Fig.10This is a comparison chart of the structural stability of the hollow spherical composite lithium adsorption materials prepared by the method (A) of Example 1 of the present invention and the method (B) of Comparative Example 2.

[0032] Fig.11 This is a physical picture of the hollow spherical composite lithium adsorption material prepared in Comparative Example 3;

[0033] Fig.12 This is a graph of the lithium adsorption performance of the hollow spherical composite lithium adsorption material prepared in Comparative Example 3. DETAILED DESCRIPTION

[0034] The present invention is further described in detail below through specific examples. The following examples are only illustrative and not restrictive, and the protection scope of the present invention cannot be limited thereto.

[0035] Example 1

[0036] A method for forming a hollow spherical composite lithium adsorption material, the specific operation is:

[0037] (1) adding 4.0 wt% of titanium-based lithium ion sieve and 0.1 wt% of hydrochloric acid-dopamine to a low-boiling-point solvent, dichloromethane, and dispersing the powdered lithium ion sieve for 30 minutes under 500 W ultrasound to obtain a suspension;

[0038] (2) adding 4.0 wt % of polysulfone to the suspension prepared in step (1), stirring at room temperature 20° C. for 5 h to prepare a casting solution;

[0039] (3) The casting solution prepared in step (2) was sucked into a syringe, and pure water was used as a receiving liquid. The casting solution was dripped dropwise at a height of 20 cm above the receiving liquid surface. After 1 hour of phase inversion, the casting solution was fully washed with pure water to obtain a hollow spherical composite lithium adsorption material (HTO / DA / PSf) (see Appendix 1). Figure 1 ), the average particle size is 1.5 to 2.5 mm (see attached Figure 2 ).

[0040] Figure 3 The HTO / DA / PSf in the composition refers to a hollow spherical composite lithium adsorption material containing a hydrophilically modified titanium-based lithium ion sieve, wherein HTO refers to a titanium-based lithium ion sieve; DA refers to a hydrophilic modifier - dopamine; and PSf refers to a polysulfone coating material.

[0041] Application Example 1

[0042] The hollow spherical composite lithium adsorbent obtained in Example 1 was dispersed in 25.0 mg L -1 The equilibrium adsorption capacity of lithium-containing solution was calculated to be 25.68 mg g at 298.15 K using inductively coupled plasma emission spectrometry. -1 (See attached Figure 3 ), which is equivalent to powder lithium ion sieve.

[0043] Example 2

[0044] A method for forming a hollow spherical composite lithium adsorption material, the specific operation is:

[0045] (1) adding 4.0 wt% of titanium-based lithium ion sieve and 0.1 wt% of hydrochloric acid-dopamine to a low-boiling-point solvent, dichloromethane, and dispersing the powdered lithium ion sieve for 30 minutes under 500 W ultrasound to obtain a suspension;

[0046] (2) adding 4.0 wt % of polysulfone to the suspension prepared in step (1), and stirring at room temperature 20°C for 3 h to prepare a casting solution;

[0047] (3) The casting solution prepared in step (2) was sucked into a syringe, and a co-solvent of ethanol and water in a volume ratio of 2:98 was used as a receiving solution. The casting solution in (2) was dripped dropwise at a height of 15 cm above the receiving solution surface. After 2 hours of phase inversion, the hollow spherical composite lithium adsorption material was obtained (see attached Figure 4 ).

[0048] Application Example 2

[0049] The hollow spherical composite lithium adsorbent obtained in Example 2 was dispersed in 25.0 mg·L -1 The equilibrium adsorption capacity of lithium-containing solution was calculated to be 25.71 mg·g at 298.15 K using inductively coupled plasma emission spectrometry. -1 (See attached Figure 5 ).

[0050] Example 3

[0051] A method for forming a hollow spherical composite lithium adsorption material, the specific operation is:

[0052] (1) adding 5.0 wt% of titanium-based lithium ion sieve and 0.1 wt% of m-phenylenediamine to a low-boiling-point solvent, dichloromethane, and dispersing the powdered lithium ion sieve for 30 minutes under 500 W ultrasound to obtain a suspension;

[0053] (2) adding 4.0 wt % of polysulfone to the suspension prepared in step (1), and stirring at room temperature 20°C for 5 h to prepare a casting solution;

[0054] (3) The casting solution prepared in step (2) was sucked into a syringe, and pure water was used as a receiving liquid. The casting solution in (2) was dripped dropwise at a height of 20 cm above the receiving liquid surface. After 2 hours of phase conversion, the hollow spherical composite lithium adsorption material (HTO / MPD / PSf) was obtained (see Figure 6 ).

[0055] Figure 6 HTO / MPD / PSf refers to a hollow spherical composite lithium adsorption material containing a hydrophilically modified titanium-based lithium ion sieve, wherein HTO refers to a titanium-based lithium ion sieve; MPD refers to a hydrophilic modifier - metaphenylenediamine; and PSf refers to a polysulfone coating material.

[0056] Application Example 3

[0057] The hollow spherical composite lithium adsorbent obtained in Example 2 was dispersed in 25.0 mg·L -1 The equilibrium adsorption capacity of lithium-containing solution was calculated to be 24.55 mg g at 298.15 K using inductively coupled plasma emission spectrometry. -1 (See attached Figure 6 ).

[0058] Comparative Example 1

[0059] In order to highlight the better performance of the hollow spherical lithium composite adsorption material prepared by this method, the existing breathing pattern method was used to prepare a flat mixed matrix lithium adsorption material. The specific steps and results are as follows:

[0060] (1) At 298.15 K, 1.0 g of titanium-based lithium ion sieve was placed in a 0.1 wt% dopamine-Tris solution with a pH of 8.50 for 5 h, washed thoroughly with deionized water until the supernatant was clear and transparent and the total organic carbon content was 0, and dried at 333.15 K;

[0061] (2) adding 4.0 wt% of the dopamine-modified lithium ion sieve powder in (1) into a low-boiling-point solvent, dichloromethane, and dispersing the lithium ion sieve powder under 500 W ultrasound for 30 minutes;

[0062] (3) adding 4.0 wt % of polysulfone to the suspension prepared in step (2), and stirring at room temperature 20°C for 5 h;

[0063] (4) A 300-mesh nylon screen was immersed in the casting solution, and a flat mixed matrix lithium adsorption material was prepared by a breathing pattern method under the conditions of 90% humidity and 293.15K.

[0064] Application Comparative Example 1

[0065] At 298.15K, the planar mixed matrix lithium adsorption material obtained in Comparative Example 1 was placed in a solution of pH = 12.0 and Li + The initial concentration was 25.0 mg·L -1The adsorption capacity of the adsorbent was calculated to be 22.18 mg·g at 298.15 K using an inductively coupled plasma emission spectrometer. -1 (See attached Figure 7 ), which is lower than the performance of the hollow spherical lithium composite adsorption material prepared by this method (equilibrium adsorption capacity is 25.68 mg·g -1 ).

[0066] Comparative Example 2

[0067] A method for forming a hollow spherical composite lithium adsorption material, the specific operations are as follows:

[0068] (1) 4.0 wt% of titanium-based lithium ion sieve was directly added to a low-boiling-point solvent, dichloromethane, without hydrophilic functional modification, and the powdered lithium ion sieve was dispersed for 30 minutes under 500 W ultrasound;

[0069] (2) adding 4.0 wt % of polysulfone to the suspension prepared in step (1), and stirring at room temperature 20°C for 5 h;

[0070] (3) The casting solution prepared in step (2) was sucked into a syringe, and pure water was used as a receiving liquid. The casting solution in (2) was dripped dropwise at a height of 20 cm above the receiving liquid surface. After 1 hour of phase inversion, the casting solution was fully washed with pure water to obtain a hollow spherical composite lithium adsorption material (HTO / PSf) (see Appendix 1). Figure 8 ).

[0071] Fig. 9 HTO / PSf refers to a hollow spherical composite lithium adsorption material containing a titanium-based lithium ion sieve that has not been hydrophilically modified, wherein HTO refers to a titanium-based lithium ion sieve and PSf refers to a polysulfone coated material.

[0072] Application Comparative Example 2

[0073] The hollow spherical composite lithium adsorbent obtained in Comparative Example 2 was dispersed in 25.0 mg·L -1 The adsorption of lithium-containing solution was completed. The equilibrium adsorption capacity at 298.15K was calculated by inductively coupled plasma emission spectrometry and was only 17.76 mg g -1 (See attached Fig. 9 However, due to the lack of interface interaction between the powder ion sieve and polysulfone, the powder ion sieve in the hollow spherical composite lithium adsorption material leaked seriously during adsorption equilibrium (see Appendix Fig.10 ), indicating that the structural stability is poor, which is not as good as the hollow spherical composite lithium adsorption material prepared by this method.

[0074] Comparative Example 3

[0075] The only difference from Example 1 is that in step (3), the co-solvent having a volume ratio of ethanol to water of 22:78 is used as the receiving liquid.

[0076] Fig.11 This is a physical picture of the hollow spherical composite lithium adsorption material prepared in Comparative Example 3. When the ethanol content exceeds 20%, the thickness of the sphere wall is too small and becomes a deflated sheet.

[0077] Application Comparative Example 3

[0078] The hollow spherical composite lithium adsorption material prepared in Comparative Example 3 was dispersed in 25.0 mg·L -1 The lithium-containing solution was tested by inductively coupled plasma emission spectrometry and its equilibrium adsorption capacity at 298.15K was calculated to be 19.90 mg g -1 (See attached Fig.12 ), the adsorption effect is far inferior to that of Example 1.

[0079] The above description is only a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several modifications and improvements without departing from the inventive concept, which all belong to the protection scope of the present invention.

Claims

1. A method for forming a hollow spherical composite lithium adsorption material, It is characterized in that The molding method is prepared by using solvent volatilization to induce phase transformation, and the specific operation is: (1) adding 1.0-6.0 wt% of lithium ion sieve powder and 0.05-0.2 wt% of catecholamine compounds to a low boiling point solvent, dispersing the lithium ion sieve powder under 400-600 W ultrasound for 20-40 minutes to obtain a suspension; (2) adding 2.0-6.0 wt % of polysulfone to the suspension, stirring for 2-5 h at room temperature of 20-25° C., to prepare a casting solution; (3) The casting liquid prepared in step (2) is sucked into a syringe, and water + ethanol co-solvent is used as a receiving liquid, the volume of ethanol in the receiving liquid is 0-20%, and the casting liquid is dripped dropwise at a height of 10-20 cm above the liquid surface of the receiving liquid. After 1-2 hours of phase conversion, it is fully washed with pure water to obtain a hollow spherical composite lithium adsorption material.

2. The molding method according to claim 1, It is characterized in that The content of polysulfone in the casting solution is 3.0-5.0 wt%.

3. The molding method according to claim 1, It is characterized in that The volume of ethanol in the receiving solution is 0-10.0%.

4. The molding method according to claim 1, It is characterized in that The catecholamine compound is one or more of dopamine hydrochloride, catechol, tannic acid, gallic acid and m-phenylenediamine.

5. The molding method according to claim 1, It is characterized in that The low boiling point solvent is one or more of dichloromethane, carbon disulfide, chloroform and tetrahydrofuran.

6. The molding method according to claim 1, It is characterized in that The polysulfone may also be polyvinyl chloride or polyvinylidene fluoride.

7. Use of the hollow spherical composite lithium adsorption material prepared by the molding method according to any one of claims 1 to 6 in adsorbing lithium.

8. The use according to claim 7, It is characterized in that The hollow spherical composite lithium adsorption material is dispersed in a lithium-containing solution with a pH of 11.5 to 12.5 at a solid-liquid ratio of 1:100 to 1:200, and the adsorption capacity is tested by an inductively coupled plasma emission spectrometer.

Citation Information

Patent Citations

  • Polyvinylidene fluoride / polydopamine modified nanometer kaolin hollow fiber composite film preparation method

    CN105233705A

  • Preparation method of composite adsorbent and method for extracting lithium from brine

    CN109225121A

  • Prussian blue composite adsorbent for selectively extracting cesium as well as preparation method and application of Prussian blue composite adsorbent

    CN117299097A

  • Spherical combined lithium adsorbent and granulation method therefor

    WO2024113501A1