Two-component rain night marking paint and preparation method thereof

Through the design of two-component coatings, methyl methacrylate resin, glass microbeads and nanosilicon dioxide are used, combined with epoxy resin microcapsules, the problem of insufficient durability of marking paint on rainy nights is solved and the marking is improved The weather resistance and night reflection effect ensure the safety of road traffic.

CN118879148APending Publication Date: 2024-11-01四川路桥高速公路养护有限公司
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411073194.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing rainy night marking paint is not durable under harsh climate conditions and is susceptible to aging caused by strong sunlight and ultraviolet radiation during the day. The reflection effect at night is reduced, affecting driving safety.

Method used

Two-component coating is used, component A includes methyl methacrylate resin, glass microbeads, nanosilica and additives, component B includes formyl peroxide, acetophenone peroxide, epoxy resin microcapsules, etc. , the weather resistance, wear resistance and self-healing ability of the coating is improved through the combination of these materials.

Benefits of technology

It significantly improves the durability of markings in harsh climates and reflective night time, extends the service life of the paint, and ensures the safety of road traffic and the clarity of markings.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of coatings, and particularly discloses a two-component rain night marking coating and a preparation method thereof. The two-component rain night marking paint comprises a component A and a component B. The component A comprises, by weight, 30-50 parts of methyl methacrylate resin, 20-30 parts of glass beads, 5-15 parts of nano-silica and 10-20 parts of an auxiliary agent. The component B is prepared from the following components in parts by weight: 20 to 30 parts of formyl peroxide, 10 to 20 parts of acetophenone peroxide, 5 to 10 parts of diisopropyl phenol, 4 to 8 parts of trichloroboric acid, 1 to 3 parts of dibutyltin dilaurate and 20 to 30 parts of quartz sand powder. The two-component rain night marking paint has the advantage that the durability of the rain night marking paint is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of coatings, and more specifically, to a two-component rainy night road marking coating and a preparation method thereof. Background Art

[0002] With the increasing traffic on the roads, the visibility and durability of road markings have become the key factors to ensure driving safety. Especially in bad weather conditions such as rainy nights, the clarity of road markings directly affects the driver's judgment and driving safety. Therefore, the rainy night marking paint technology came into being. Through unique materials and process design, it effectively improves the visibility of road markings in bad weather, thus ensuring the safety and smoothness of road traffic.

[0003] The core technology of Rainy Night Road Marking Paint lies in the new materials and unique reflective principle. The reflective effect of traditional road markings will be greatly reduced on rainy days or at night due to rain erosion and insufficient light, making it difficult for drivers to identify. Rainy Night Road Marking Paint uses special Rainy Night reflective beads and high-performance paint, so that the markings can still maintain a high-brightness reflective effect in bad weather such as rainy nights.

[0004] However, at present, the durability of road marking paints for rainy nights is insufficient under harsh climatic conditions. The strong sunlight and ultraviolet radiation during the day will cause the organic components in the paint to gradually decompose, which is an inevitable natural aging process. Long-term exposure to the sun makes the paint surface fragile and prone to cracking or peeling, further shortening the service life of the paint. At night, especially when it rains, the paint that has been exposed to the sun and aged faces erosion and penetration by rainwater. Rainwater may not only wash away the particles on the surface of the paint, but also penetrate into the paint, accelerating the peeling and splitting of the paint, thereby affecting the clarity of the markings and driving safety. Summary of the invention

[0005] In order to improve the durability of rainy night road marking paint, the present application provides a two-component rainy night road marking paint and a preparation method thereof.

[0006] In the first aspect, the two-component rainy night road marking paint provided by the present application adopts the following technical solution: A two-component rainy night road marking paint comprises a component A and a component B, wherein the component A comprises 30-50 parts of methyl methacrylate resin, 20-30 parts of glass microbeads, 5-15 parts of nano silicon dioxide and 10-20 parts of an auxiliary agent in parts by weight, and the component B comprises 20-30 parts of formyl peroxide, 10-20 parts of acetophenone peroxide, 5-10 parts of diisopropyl phenol, 4-8 parts of trichloroboric acid, 1-3 parts of dibutyltin dilaurate and 20-30 parts of quartz sand powder in parts by weight.

[0007] By adopting the above technical scheme, methyl methacrylate resin has excellent weather resistance and UV resistance, can effectively resist strong sunlight and UV radiation during the day, slow down the aging process of the coating, and improve the durability of the coating. Glass microbeads improve the visibility of the marking at night, enhance the wear resistance and pressure resistance of the coating, and extend the service life of the coating. The addition of nano-silicon dioxide can further improve the weather resistance and wear resistance of the coating. Nanomaterials have a large specific surface area and high surface activity, can form a close bond with the resin, and enhance the density and durability of the coating. Formyl peroxide and acetophenone peroxide are initiators. They initiate the polymerization reaction of the resin during the curing process of the coating to form a dense coating film, and improve the water resistance and corrosion resistance of the coating. Diisopropylphenol and trichloroboric acid can further adjust the curing speed and curing degree of the coating to ensure that the coating has excellent performance after curing. Quartz sand powder, as an inorganic filler, can improve the wear resistance and pressure resistance of the coating while reducing the cost of the coating. Through the implementation of the above technical solutions, the two-component rainy night marking paint has excellent weather resistance, UV resistance, water resistance and wear resistance, which can significantly improve the durability of the markings under adverse weather conditions.

[0008] Optionally, the component A further comprises 20-40 parts by weight of epoxy resin microcapsules.

[0009] Optionally, the preparation method of the epoxy resin microcapsules is: 40-60 parts of bisphenol A epoxy resin and 10-15 parts of trimethylol acrylate are added to a reaction vessel, emulsified and dispersed using a high shear emulsifier, 1-5 parts of sodium lauryl carboxylate are dissolved in 3-5 parts of deionized water, stirred evenly, and then added to the reaction vessel, and stirring is continued; Add 120-180 parts of urea-formaldehyde resin prepolymer, 5-10 parts of oxalyl diimidazole, 1-3 parts of resorcinol and 2-4 parts of n-butanol into a reaction container; Under stirring conditions, the pH value of the system is adjusted to 3.0-4.0 with dilute HCl, heated to 60-70°C, and reacted for 2-3 hours to form uniform microcapsules; After the reaction is completed, the wall material prepolymer that has not participated in the reaction, the remaining wall material and the uncoated core material are removed through the steps of filtering, washing and drying to obtain epoxy resin microcapsules.

[0010] By adopting the above technical scheme, the addition of epoxy resin microcapsules can significantly improve the durability of the coating. The epoxy resin in the microcapsules can be released and repair cracks or peeling parts when the coating is damaged, thereby extending the service life of the coating. This self-healing ability is particularly suitable for road marking paint on rainy nights, because the paint is easily damaged under severe weather conditions. Epoxy resin itself has good weather resistance and UV resistance. Therefore, adding epoxy resin microcapsules to the coating can further enhance the weather resistance and UV resistance of the coating, allowing it to maintain stable performance under long-term sunlight and UV radiation. Epoxy resin microcapsules have high hardness and good flexibility, which can enhance the wear resistance and compression resistance of the coating. When the coating is subjected to vehicle driving or human wear, it can better resist damage and maintain the clarity and integrity of the marking line.

[0011] Optionally, the B component further comprises 5-15 parts by weight of fluorinated ethylene-fluoropropylene copolymer.

[0012] Optionally, the B component further comprises 10-15 parts by weight of benzyl benzoate.

[0013] By adopting the above technical solution, the fluorinated ethylene-fluoropropylene copolymer has excellent chemical resistance and thermal stability, and can resist the erosion of chemicals such as acids, alkalis, solvents, as well as damage from ultraviolet rays and high temperatures. This will give the coating a longer service life under harsh climate conditions. The addition of fluorinated ethylene-fluoropropylene copolymer can increase the wear resistance and scratch resistance of the coating, making it better resistant to vehicle driving and human wear.

[0014] Benzyl benzoate can improve the adhesion between the paint and the substrate, making the paint adhere more tightly to the road surface and less likely to peel off. It may also increase the flexibility of the paint, allowing it to better adapt to the deformation and expansion of the road surface and reduce the possibility of cracking and peeling.

[0015] Optionally, the auxiliary agent includes 10-15 parts of fatty alcohol polyoxyethylene ether and 1-5 parts of sodium polyacrylate in parts by weight.

[0016] In the second aspect, the present application provides a method for preparing a two-component rainy night road marking paint, which adopts the following technical solution: A method for preparing a two-component rainy night road marking paint comprises the following steps: Add methyl methacrylate resin, glass microbeads, nano-silica and additives into a mixing container in proportion, mix and stir evenly to ensure that all components are fully mixed, and obtain component A; Add formyl peroxide, acetophenone peroxide, diisopropylphenol, trichloroboric acid, a catalyst and quartz sand powder into a mixing container in proportion, mix and stir evenly to ensure that all components are fully mixed, to obtain component B; The pre-prepared component A and component B are mixed and stirred evenly to obtain a two-component rainy night road marking paint.

[0017] Optionally, epoxy resin microcapsules are added to the component A and stirred evenly, and fluorinated ethylene-fluoropropylene copolymer and benzyl benzoate are added to the component B and stirred evenly.

[0018] By adopting the above technical solution, when the two components are mixed, the resulting coating not only has excellent weather resistance, wear resistance and adhesion, but also enhances the self-healing ability of the coating by adding epoxy resin microcapsules, and improves the corrosion resistance, flexibility and stability of the coating by adding fluorinated ethylene-fluoropropylene copolymer and benzyl benzoate. This preparation method ensures that the road marking paint can remain clear and durable under various adverse weather conditions on rainy nights, thereby greatly improving the safety of road driving. .

[0019] In summary, this application has the following beneficial effects: 1. Since the present application adopts component A, methyl methacrylate resin provides good weather resistance and film-forming properties, glass microbeads enhance the nighttime reflective effect, nano-silicon dioxide improves the wear resistance and durability of the coating, and the additives optimize the construction performance of the coating. In component B, formyl peroxide and acetophenone peroxide are used as initiators to ensure the rapid curing of the coating, diisopropylphenol and trichloroboric acid regulate the curing process, dibutyltin dilaurate is used as a catalyst to accelerate the curing reaction, and quartz sand powder enhances the wear resistance and compression resistance of the coating. This two-component rainy night marking paint not only has excellent weather resistance, wear resistance and nighttime reflective effect, but also has a fast curing speed and is easy to construct. It is suitable for various road markings to ensure driving safety.

[0020] 2. In this application, epoxy resin microcapsules are preferably added to the two-component rainy night road marking paint, which significantly enhances the durability of the paint. The epoxy resin in the microcapsules has a self-repairing function, which can be released and fill cracks or peeling parts when the paint is damaged, effectively extending the service life of the paint. This self-repairing ability is particularly important, especially in severe weather conditions. In addition, the weather resistance and UV resistance of the epoxy resin itself further enhance the stability and durability of the paint, ensuring that it can still maintain excellent performance under long-term sunlight and UV radiation.

[0021] 3. The fluorinated ethylene-fluoropropylene copolymer preferably used in this application has excellent chemical resistance and thermal stability, and can resist the erosion of chemicals such as acids, alkalis, solvents, and damage from ultraviolet rays and high temperatures. This will give the coating a longer service life under harsh climatic conditions. DETAILED DESCRIPTION

[0022] The present application is further described in detail below in conjunction with the examples. It is particularly noted that if no specific conditions are specified in the following examples, the experiments are carried out according to conventional conditions or the conditions recommended by the manufacturer. Unless otherwise specified, the raw materials used in the following examples can be obtained from common commercial sources.

[0023] Preparation Example of Epoxy Resin Microcapsules Preparation Example 1 Preparation method of epoxy resin microcapsules: 50 kg of bisphenol A epoxy resin and 15 kg of trimethylol acrylate were added to a reaction vessel, and emulsified and dispersed at a speed of 4500 r / min in a high shear emulsifier. 5 kg of sodium lauryl carboxylate was dissolved in 5 kg of deionized water, and the mixture was added to the reaction vessel after being stirred evenly, and stirring was continued; Under stirring conditions, urea and 37% formaldehyde aqueous solution are mixed in a mass ratio of 1:2, the pH value of the solution is adjusted to 8-9 with triethanolamine, the temperature is raised to 70°C, and the reaction is carried out at this temperature for 1 hour, and after cooling to room temperature, a urea-formaldehyde resin prepolymer is obtained; Add 180 kg of urea-formaldehyde resin prepolymer, 10 kg of oxalyl diimidazole, 3 kg of resorcinol and 4 kg of n-butanol into a reaction container; Under stirring conditions, the pH value of the system was adjusted to 3.0-4.0 with dilute HCl, heated to 65°C, and reacted for 3 hours to form uniform microcapsules; After the reaction is completed, the wall material prepolymer that has not participated in the reaction, the remaining wall material and the uncoated core material are removed by filtering and washing, and then vacuum drying is performed to obtain epoxy resin microcapsules.

[0024] Preparation Example 2 Preparation method of epoxy resin microcapsules: 50 kg of bisphenol A epoxy resin and 10 kg of trimethylol acrylate were added to a reaction vessel, and emulsified and dispersed at a speed of 4500 r / min in a high shear emulsifier. 1 kg of sodium lauryl carboxylate was dissolved in 3 kg of deionized water, stirred evenly, and then added to the reaction vessel, and stirring was continued; Under stirring conditions, urea and 37% formaldehyde aqueous solution are mixed in a mass ratio of 1:2, the pH value of the solution is adjusted to 8-9 with triethanolamine, the temperature is raised to 70°C, and the reaction is carried out at this temperature for 1 hour, and after cooling to room temperature, a urea-formaldehyde resin prepolymer is obtained; Add 120 kg of urea-formaldehyde resin prepolymer, 5 kg of oxalyl diimidazole, 1 kg of resorcinol and 2 kg of n-butanol into a reaction container; Under stirring conditions, the pH value of the system was adjusted to 3-4 with dilute HCl, heated to 65°C, and reacted for 3 hours to form uniform microcapsules; After the reaction is completed, the wall material prepolymer that has not participated in the reaction, the remaining wall material and the uncoated core material are removed by filtering and washing, and then vacuum drying is performed to obtain epoxy resin microcapsules.

[0025] Preparation Example 3 Preparation method of epoxy resin microcapsules: 50 kg of bisphenol A epoxy resin and 12 kg of trimethylol acrylate were added to a reaction vessel, and emulsified and dispersed at a speed of 4500 r / min in a high shear emulsifier. 3 kg of sodium lauryl carboxylate was dissolved in 4 kg of deionized water, and the mixture was added to the reaction vessel after being stirred evenly, and stirring was continued; Under stirring conditions, urea and 37% formaldehyde aqueous solution are mixed in a mass ratio of 1:2, the pH value of the solution is adjusted to 8-9 with triethanolamine, the temperature is raised to 70°C, and the reaction is carried out at this temperature for 1 hour, and after cooling to room temperature, a urea-formaldehyde resin prepolymer is obtained; Add 150 kg of urea-formaldehyde resin prepolymer, 7 kg of oxalyl diimidazole, 2 kg of resorcinol and 3 kg of n-butanol into a reaction container; Under stirring conditions, the pH value of the system was adjusted to 3.0-4.0 with dilute HCl, heated to 65°C, and reacted for 3 hours to form uniform microcapsules; After the reaction is completed, the wall material prepolymer that has not participated in the reaction, the remaining wall material and the uncoated core material are removed by filtering and washing, and then vacuum drying is performed to obtain epoxy resin microcapsules.

[0026] Preparation Example 4 Preparation method of epoxy resin microcapsules: The difference from Preparation Example 3 is that the urea-formaldehyde resin prepolymer is replaced by polyurethane. Example

[0027] Example 1 Preparation method of two-component rainy night road marking paint: 40 kg of methyl methacrylate resin, 25 kg of glass microbeads, 10 kg of nano-silica, 10.5 kg of fatty alcohol polyoxyethylene ether and 4.5 kg of sodium polyacrylate were added into a mixing container, and mixed evenly by magnetic stirring to ensure that the components were fully mixed, thereby obtaining component A; Add 25 kg of formyl peroxide, 15 kg of acetophenone peroxide, 8 kg of diisopropylphenol, 6 kg of trichloroboric acid, 2 kg of dibutyltin dilaurate and 25 kg of quartz sand powder into a mixing container, stir evenly to ensure that all components are fully mixed, to obtain component B; The pre-prepared component A and component B were mixed, and stirred at a speed of 120 r / min for 15 min by a stirrer to obtain a two-component rainy night road marking paint.

[0028] Example 2 Preparation method of two-component rainy night road marking paint: The difference from Example 1 is that 30 kg of epoxy resin microcapsules are also added to component A and stirred, and the epoxy resin microcapsules are prepared by Preparation Example 1.

[0029] Example 3 Preparation method of two-component rainy night road marking paint: The difference from Example 1 is that 30 kg of epoxy resin microcapsules are also added to component A and stirred, and the epoxy resin microcapsules are prepared by Preparation Example 2.

[0030] Example 4 Preparation method of two-component rainy night road marking paint: The difference from Example 1 is that 30 kg of epoxy resin microcapsules are also added to component A and stirred, and the epoxy resin microcapsules are prepared by Preparation Example 3.

[0031] Example 5 Preparation method of two-component rainy night road marking paint: The difference from Example 4 is that 10 kg of fluorinated ethylene-fluoropropylene copolymer is also added to component B, and the fluorinated ethylene-fluoropropylene copolymer is purchased from DuPont in the United States.

[0032] Example 6 Preparation method of two-component rainy night road marking paint: The difference from Example 4 is that 12 kg of benzyl benzoate is also added to component B, and benzyl benzoate is purchased from Jiangsu Tiancheng Chemical.

[0033] Comparative Example Comparative Example 1 Preparation method of two-component rainy night road marking paint: The difference from Example 4 is that 30 kg of epoxy resin microcapsules are also added to component A and stirred, and the epoxy resin microcapsules are prepared by Preparation Example 4.

[0034] Comparative Example 2 Preparation method of two-component rainy night road marking paint: The difference from Example 4 is that 30 kg of analytically pure epoxy resin is also added to component A and stirred.

[0035] Comparative Example 3 Preparation method of two-component rainy night road marking paint: The difference from Example 4 is that the methyl methacrylate resin in component A is replaced by acrylic resin, and the acrylic resin is purchased from Mitsubishi acrylic resin MB-2660 of Japan.

[0036] Performance testing Detection Methods A xenon arc lamp aging tester was used to conduct an artificial accelerated aging test on the 3mm thick paint after drying and curing. Under the conditions of 30℃ and 50% humidity, the xenon arc lamp was used for 12 hours every day. After irradiation, the temperature was lowered to 10℃ and kept warm for 4 hours. The paint was washed by a spray system simulating a precipitation rate of 5mm / h. After 4 hours, the spraying was stopped and left for 4 hours. This 24-hour cycle was repeated. After 10 days of circulation, the adhesion of the paint was tested, the wear test of the 60-mesh grinding wheel was performed, and the coating was observed for cracks and damage.

[0037] Table 1 Test data statistics Adhesion / MPa Wear test / cycle Coating appearance Example 1 2.23 223 No cracks, no damage Example 2 3.43 238 No cracks, no damage Example 3 3.40 243 No cracks, no damage Example 4 3.57 248 No cracks, no damage Example 5 3.61 265 No cracks, no damage Example 6 3.78 253 No cracks, no damage Comparative Example 1 3.38 240 There is cracking Comparative Example 2 3.25 232 There is cracking Comparative Example 3 3.33 238 There is cracking Combining Example 4 and Comparative Example 1 and Table 1, it can be seen that in Preparation Example 4, urea-formaldehyde resin prepolymer is not used as the wall material, but polyurethane is used. The durability of the resulting coating is far inferior to that of Example 4 as can be seen from the test results.

[0038] Combining Example 4 and Comparative Example 2 with Table 1, it can be seen that in Comparative Example 2, epoxy resin is directly used instead of microencapsulated epoxy resin. This shows that the addition of epoxy resin microcapsules can significantly improve the durability of the coating.

[0039] Combining Example 4 and Comparative Example 3 with Table 1, it can be seen that methyl methacrylate resin has excellent weather resistance and UV resistance, can effectively resist strong sunlight and UV radiation during the day, slow down the aging process of the coating, and improve the durability of the coating.

[0040] It can be seen from Examples 1-4 and Table 1 that adding epoxy resin microcapsules to the coating can further enhance the weather resistance and UV resistance of the coating, enabling it to maintain stable performance under long-term sunlight and UV radiation. The epoxy resin microcapsules have high hardness and good flexibility, which can enhance the wear resistance of the coating. The epoxy resin microcapsules obtained in Preparation Example 3 are the best.

[0041] It can be seen from Examples 4-6 and Table 1 that the addition of fluorinated ethylene-fluorinated propylene copolymer can increase the wear resistance and scratch resistance of the coating, making it more resistant to vehicle driving and human wear. Benzyl benzoate can improve the adhesion between the coating and the substrate, making the coating adhere more closely to the road surface and not easy to peel off.

[0042] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A two-component rainy night road marking paint, characterized in that: The invention comprises component A and component B, wherein component A comprises 30-50 parts of methyl methacrylate resin, 20-30 parts of glass microspheres, 5-15 parts of nano silicon dioxide and 10-20 parts of auxiliary agent in parts by weight, and component B comprises 20-30 parts of formyl peroxide, 10-20 parts of acetophenone peroxide, 5-10 parts of diisopropyl phenol, 4-8 parts of trichloroboric acid, 1-3 parts of dibutyltin dilaurate and 20-30 parts of quartz sand powder in parts by weight.

2. The two-component rainy night road marking paint according to claim 1, characterized in that: The component A also includes 20-40 parts by weight of epoxy resin microcapsules.

3. The two-component rainy night road marking paint according to claim 2 is characterized in that: The preparation method of the epoxy resin microcapsule is: 40-60 parts of bisphenol A epoxy resin and 10-15 parts of trimethylol acrylate are added to a reaction vessel, emulsified and dispersed using a high shear emulsifier, 1-5 parts of sodium lauryl carboxylate are dissolved in 3-5 parts of deionized water, stirred evenly, and then added to the reaction vessel, and stirring is continued; Add 120-180 parts of urea-formaldehyde resin prepolymer, 5-10 parts of oxalyl diimidazole, 1-3 parts of resorcinol and 2-4 parts of n-butanol into a reaction container; Under stirring conditions, the pH value of the system is adjusted to 3.0-4.0 with dilute HCl, heated to 60-70°C, and reacted for 2-3 hours to form uniform microcapsules; After the reaction is completed, the wall material prepolymer that has not participated in the reaction, the remaining wall material and the uncoated core material are removed through the steps of filtering, washing and drying to obtain epoxy resin microcapsules.

4. The two-component rainy night road marking paint according to claim 1, characterized in that: The B component also includes 5-15 parts by weight of fluorinated ethylene-fluoropropylene copolymer.

5. The two-component rainy night road marking paint according to claim 1, characterized in that: The B component also includes 10-15 parts by weight of benzyl benzoate.

6. The two-component rainy night road marking paint according to claim 1, characterized in that: The auxiliary agent comprises fatty alcohol polyoxyethylene ether and sodium polyacrylate in a mass ratio of 7:

3.

7. A method for preparing a two-component rainy night road marking paint as claimed in any one of claims 1 to 6, characterized in that: The following steps are involved: Add methyl methacrylate resin, glass microbeads, nano-silica and additives into a mixing container in proportion, mix and stir evenly to ensure that all components are fully mixed, and obtain component A; Add formyl peroxide, acetophenone peroxide, diisopropylphenol, trichloroboric acid, a catalyst and quartz sand powder into a mixing container in proportion, mix and stir evenly to ensure that all components are fully mixed, to obtain component B; The pre-prepared component A and component B are mixed and stirred evenly to obtain a two-component rainy night road marking paint.

8. The method for preparing the two-component rainy night road marking paint according to claim 7, characterized in that: Epoxy resin microcapsules are added to the component A and stirred evenly, and fluorinated ethylene-fluorinated propylene copolymer and benzyl benzoate are added to the component B and stirred evenly.

Citation Information

Patent Citations

  • High speed drying paint composition for marking road line and preparation process thereof

    KR1020100079867A

  • The vehicle's side airbag system protecting a passenger in the full position during a side collision

    KR1020250068920A

  • Multi-layer cosmetic composition using the repulsion between alkyl polyglucosides and ingredients

    KR1020260030292A

  • Dedicated de-ferment device for secondary battery raw materials

    KR102212474B1

  • A room temperature curing paint composition for lane painting

    KR102539197B1