Explosion-proof polyurea material and preparation method thereof
By combining chemically modified aramid fibers with specific resin components, explosion-proof polyurea materials with high tensile properties and tear resistance are prepared, solving the problem of poor tear resistance under high-speed impact. And maintains the convenience of spraying construction.
Patent Information
- Application Number
- CN202411069732.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-08-06
AI Technical Summary
Existing polyurea materials are difficult to achieve good tear resistance under high-speed impact, and conventional methods such as increasing hard segment content or filler will lead to poor low-temperature flexibility or difficulty in spraying.
Using chemical modification methods, chlorine activated modified aramid fibers with amino and carboxyl groups, hexamethylene diisocyanate, catalyst, polyol and polyisocyanate, are used to prepare explosion-proof poly through efficient reaction and drying steps. Urea material, improves the tensile properties and tear resistance of the material.
显著提高了聚脲材料的拉伸性能和抗撕裂能力,满足防爆和防弹要求,同时不影响喷涂施工效果,并避免堵枪现象。
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polyurea production and processing, and specifically relates to an explosion-proof polyurea material and a preparation method thereof. Background Art
[0002] Spray polyurea materials are widely used in the fields of submarine pipelines, buried pipeline anti-corrosion, storage tank anti-corrosion, concrete protection, waterproofing, military skin, chassis protection, etc. due to their solvent-free and environmentally friendly, high mechanical strength, and fast construction. For example, polyurea materials can be used for the protection of hazardous chemical vehicles, and their coatings have high impact resistance and explosion resistance. When the vehicle body burns, the coating can seal, reduce the entry of external oxygen and prevent the expansion of combustion; at the same time, when the explosion occurs, the coating can absorb and block the explosion shock wave to protect the lives of drivers and passengers. It can also be used for petrochemical explosion-proof buildings: In the field of petrochemicals, spray polyurea technology is used in the construction of explosion-proof buildings. This coating can alleviate shock waves during explosions, prevent building debris from splashing, reduce damage to buildings caused by explosions, and protect the safety of people and property in buildings. It can also be used for the protection of public places and tunnels: Spray polyurea materials are also used for the protection of enclosed spaces such as public places and tunnels. Setting up explosion-proof walls, explosion-proof doors and explosion-proof barriers made of polyurea materials in these places can effectively prevent the propagation of deflagration shock waves and reduce casualties and property losses. In addition, spray polyurea materials also play an important role in bulletproof applications. The application of spray polyurea technology in bulletproof inserts is mainly reflected in its enhanced bulletproof function. The polyurea coating sprayed on the surface of ceramic plates or PE plates can reduce the fragmentation of ceramic plates and increase the ability to resist multiple bullets. This coating, combined with repairable explosion-proof and bulletproof materials, can bond ceramic plates and PE plates together at room temperature without gaps, reduce bullet speed, and play the role of waterproof, wear-resistant, anti-fall and cracking, beautiful, and prolong service life. In the field of military bulletproof and explosion-proof protective materials, in addition to requiring the coating itself to have ultra-high physical strength, it is also required to show good tear resistance under high-speed impact, but conventional polyurea products are difficult to meet the above requirements.
[0003] Polyurea has many formulas and a wide range of applications. Different formulas and preparation methods should be used to adapt to its application field according to its use. The current conventional solution is to add special fillers to the polyurea resin system or to use a pure polyurea system and improve the performance by increasing the hard segment content. The former physical blending method has poor dispersibility, and the addition of fillers makes polyurea spraying difficult. Moreover, if too much filler is added, the material is prone to separation of filler and resin under high-speed impact, which is manifested as a sharp drop in coating strength under high-speed impact; the latter increases the hard segment content of the resin, although it increases the strength of the material, but its hardness is also greatly increased, resulting in poor low-temperature flexibility of the material, and the material loses its anti-ballistic and explosion-proof function under low-temperature environments.
[0004] In addition to the basic characteristics of high-performance fibers, aramid fibers also have the advantages of flame retardancy and fatigue resistance. Since they were discovered by DuPont, they have been valued and developed. Aramid fiber-resin composite materials have good application prospects in the field of composite matrix reinforcement processing due to their excellent performance in impact resistance, fracture elongation and damage tolerance.
[0005] At present, the main problem facing the performance of aramid fiber reinforced composite matrix is the interface compatibility between aramid fiber and composite material. Aramid fiber is a long straight chain structure composed of alternating amide bonds and aromatic rings. Due to the highly symmetrical molecular structure, it has the characteristics of high orientation and high crystallinity, and the surface is very smooth. At the same time, the presence of benzene rings on the molecular chain also brings a large steric effect, which makes the surface of aramid fiber lack active groups. Combining these two reasons, the interfacial bonding performance between aramid fiber and resin matrix is very poor. In actual use, it is affected by external factors, which easily leads to fiber pull-out and detachment, causing fiber failure. Summary of the invention
[0006] The object of the present invention is to provide an explosion-proof polyurea material and a preparation method thereof to solve the problems raised in the above background technology.
[0007] To achieve the above object, the present invention provides the following technical solutions:
[0008] The raw materials for preparing an explosion-proof polyurea material include component A and component B. The raw materials of component A include chlorine-activated modified aramid fiber with amino and carboxyl groups.
[0009] Preferably, the structural formula of the modified aramid fiber is:
[0010]
[0011] Preferably, the raw materials of component A also include hexamethylene diisocyanate, a catalyst, a polyol and a polyisocyanate;
[0012] The raw materials of the modified aramid fiber include nano-aramid fiber and sodium dichloroisocyanurate.
[0013] Preferably, the preparation steps of component A include:
[0014] (1) adding an appropriate amount of nano-aramid fiber to an appropriate amount of sodium dichloroisocyanurate aqueous solution, adding an appropriate amount of hydrochloric acid after the reaction is completed, heating, purifying and drying to obtain modified aramid fiber;
[0015] (2) mixing an appropriate amount of modified aramid fiber, hexamethylene diisocyanate and a catalyst, and after the reaction is completed, purifying and drying to obtain an intermediate product 1;
[0016]
[0017] (3) Pre-treating the polyol, then adding an appropriate amount of polyisocyanate, and after the reaction is completed, adding the intermediate product 1 to obtain component A.
[0018] Preferably, the mass ratio of the nano-aramid fiber to the 50% sodium dichloroisocyanurate aqueous solution is 0.1-1:250-350 parts, and the concentration of the sodium dichloroisocyanurate aqueous solution is 50%;
[0019] The mass ratio of modified aramid fiber, hexamethylene diisocyanate and catalyst in the raw materials of component A is 1-2:25-35:0-0.1;
[0020] The mass ratio of polyol, polyisocyanate and intermediate product 1 in the raw materials of component A is 50-100:100-250:150-350.
[0021] Preferably,
[0022] The process conditions of step (1) are as follows: the nano-aramid fiber is added to the sodium dichloroisocyanurate aqueous solution and dispersed and mixed at a speed of 2000-3000 r / min for 2-8 minutes, filtered to remove water, reacted in an oven at 50-80° C. for 1-5 hours, heated at 100-120° C. for 1-2 hours after adding the hydrochloric acid solution, the product is washed with deionized water, and finally dried in an oven at 90-110° C. for 6-8 hours;
[0023] The process conditions of step (2) are to stir and ultrasonically react for 8-15 hours in a closed nitrogen environment at room temperature, and after the reaction is completed, use hexane to clean the residual HDI on the surface to ensure that the solvent on the surface of the nano-aramid fiber is cleaned, and finally dry at 50-60° C. for use;
[0024] The pretreatment process conditions of step (3) are to heat the polyol to 95-105°C with stirring, dehydrate for 5-7h, release the vacuum, and cool to below 50°C; the reaction process conditions are to add the polyisocyanate, react at 80-100°C for 3-4h, then add 3-10 parts of the intermediate product 1 and continue stirring for 4-6h.
[0025] Preferably, the mass ratio of the amino-terminated polyether, the polyol, the coupling agent, the chain extender, the catalyst, the water scavenger and the color paste is 30-60:20-50:1-2:20-40:0-1:1-5:1-5.
[0026] Preferably, the catalyst includes one or more of bismuth isooctanoate, zinc isooctanoate, triethylenediamine, bismorpholinyl diethyl ether, tetrabutyl borate, and tetraisopropyl borate.
[0027] Preferably, the purity of the nano-aramid fiber is ≥99% and the specific surface area is 7–11 m 2 / g.
[0028] Preferably, the -NCO content of the isocyanate prepolymer of component A is 14% to 17%; and the isocyanate index of components A and B is 1.05 to 1.10.
[0029] Preferably, the polyisocyanate is one or more of diphenylmethane diisocyanate, isophorone diisocyanate, dicyclohexylmethane diisocyanate, methylcyclohexyl diisocyanate, cyclohexane dimethylene diisocyanate, xylylene diisocyanate, and 1,4-cyclohexane diisocyanate.
[0030] Preferably, the amino-terminated polyether includes one or more of difunctional amino-terminated polyether and trifunctional amino-terminated polyether.
[0031] Preferably, the polyol is one or more of polyoxypropylene diol, polytetramethylene glycol, polycaprolactone diol, polyester diol, and polycarbonate diol, and the average molecular weight of the polyol is 400-1500, the water content is ≤0.5%, and the acid value is ≤0.8 mg KOH / g.
[0032] Preferably, the coupling agent is one or more of a silane coupling agent, a borate coupling agent, an aluminate coupling agent, a borate coupling agent, a bimetallic coupling agent, and a phosphate coupling agent.
[0033] Preferably, the dehydrating agent is a molecular sieve, and the specification of the molecular sieve is 3a or 4a.
[0034] Preferably, the chain extender includes 3,5-dimethylthiotoluenediamine, 2,4-diamino-3,5-dimethylthiochlorobenzene, 4,4′-bis-sec-butylaminodiphenylmethane, N,N,-dialkylphenylenediamine, 2,4-diamino-3-methylthio-5-propyltoluene, 3,3′-dimethyl-4,4′-diaminodicyclohexylmethane, 4,4,-bis-sec-butylaminodicyclohexylmethane, 3,3,-dimethyl-4,4,-bis-sec-butylamino-dicyclohexylmethane, trimethylhexanediamine or hydrogenated MDA.
[0035] Preferably, the color paste is a general color paste in the polyurethane industry, and its color includes one of red, yellow, blue, green, white and black, and the water content of the color paste is ≤0.5%.
[0036] A method for preparing an explosion-proof polyurea material comprises the following steps:
[0037] (1) adding an appropriate amount of nano-aramid fiber to an aqueous solution of sodium dichloroisocyanurate, purifying and drying after the reaction is completed, adding hydrochloric acid, and heating to obtain modified aramid fiber;
[0038] (2) mixing an appropriate amount of modified aramid fiber, hexamethylene diisocyanate and a catalyst, and after the reaction is completed, purifying and drying to obtain an intermediate product 1;
[0039] (3) pre-treating the polyol, then adding an appropriate amount of polyisocyanate to obtain a component A after the reaction is completed; and then adding the intermediate product 1;
[0040] (4) mixing appropriate amounts of amino-terminated polyether, polyol, coupling agent, chain extender, catalyst, water scavenger and color paste to obtain component B;
[0041] (5) Mix appropriate amounts of component A and component B to obtain an explosion-proof polyurea material.
[0042] Preferably, the volume ratio of component A to component B is 1:1.
[0043] Preferably, the process conditions of step (1) are as follows: the nano-aramid fiber is added to the sodium dichloroisocyanurate aqueous solution and dispersed and mixed at a speed of 2000-3000 r / min for 2-8 min, filtered to remove water, reacted in an oven at 50-80° C. for 1-5 hours, heated at 100-120° C. for 1-2 hours after adding the hydrochloric acid solution, the product is washed with deionized water, and finally dried in an oven at 90-110° C. for 6-8 hours;
[0044] Preferably, the process conditions of step (2) are stirring and ultrasonically reacting for 8-15 hours in a closed nitrogen environment at room temperature, and after the reaction is completed, washing the residual HDI on the surface with hexane to ensure that the solvent on the surface of the aramid fiber is cleaned, and finally drying at 50-60° C. for use;
[0045] Preferably, the pretreatment process conditions of step (3) are to heat the polyol to 95-105° C. with stirring, dehydrate for 5-7 hours, release the vacuum, and cool to below 50° C.; the reaction process conditions are to add the polyisocyanate and react at 80-100° C. for 3-4 hours, then add the intermediate 1 and continue stirring for 4-6 hours;
[0046] Preferably, the process conditions of step (4) are to stir, grind and filter the raw materials of component B.
[0047] Compared with the prior art, the present invention has the following beneficial effects:
[0048] The present invention greatly improves the tensile properties and tear resistance of the polyurea material. The present invention adopts a chemical modification method for preparation, which is different from the modification of aramid fiber and polyurea by physical blending. The polyurea material prepared by the present invention has extremely high tear strength. Under the premise of meeting the requirements of explosion-proof and bullet-proof, it does not affect the construction effect of spraying and will not cause gun clogging. DETAILED DESCRIPTION
[0049] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0050] Embodiment 1:
[0051] (1) 0.1 parts of nano-aramid fiber was added to 250 parts of a 50% sodium dichloroisocyanurate aqueous solution, and the mixture was dispersed and mixed at a speed of 2000 r / min for 2 min. After the water was removed by filtration, the mixture was reacted in a 50° C. oven for 1 hour. After the hydrochloric acid solution was added, the mixture was heated at 100° C. for 1 hour. The product was washed with deionized water, and finally dried in a 90° C. oven for 6 hours to obtain modified aramid fiber.
[0052] (2) 1 part of modified aramid fiber and 25 parts of hexamethylene diisocyanate were mixed and stirred for ultrasonic reaction in a closed nitrogen environment at room temperature for 8 hours. After the reaction, the residual HDI on the surface was cleaned with hexane to ensure that the solvent on the surface of the aramid fiber was cleaned. Finally, the fiber was dried at 50°C for use to obtain an intermediate product 1.
[0053] (3) 50 parts of polyoxypropylene glycol were heated to 95° C. with stirring, dehydrated for 5 h, released from vacuum, cooled to below 50° C., then 150 parts of diphenylmethane diisocyanate were added and reacted at 80° C. for 3 h, 3 parts of intermediate product 1 were added and stirred for 4 h to obtain component A;
[0054] (4) 30 parts of difunctional amino-terminated polyether, 20 parts of polyoxypropylene glycol, 1 part of silane coupling agent, 20 parts of 3,5-dimethylthiotoluenediamine, 1 part of molecular sieve with specification 3a and 1 part of color paste are stirred, ground and filtered to obtain component B;
[0055] (5) Component A and component B are mixed in a volume ratio of 1:1 to obtain an explosion-proof polyurea material.
[0056] Embodiment 2:
[0057] (1) adding 1 part of nano-aramid fiber to 350 parts of 50% sodium dichloroisocyanurate aqueous solution, and dispersing and mixing at a speed of 3000 r / min for 8 min, filtering to remove water, reacting in an oven at 80° C. for 5 h, adding hydrochloric acid solution, heating at 120° C. for 2 h, washing the product with deionized water, and finally drying in an oven at 110° C. for 8 h to obtain modified aramid fiber;
[0058] (2) 2 parts of modified aramid fiber, 35 parts of hexamethylene diisocyanate, 0.1 parts of zinc isooctanoate, 0.03 parts of triethylenediamine, and 0.01 parts of dimorpholino diethyl ether were mixed and stirred for ultrasonic reaction in a closed nitrogen environment at room temperature for 15 hours. After the reaction, the residual HDI on the surface was cleaned with hexane to ensure that the solvent on the surface of the aramid fiber was cleaned. Finally, the fiber was dried at 60°C for use to obtain an intermediate product 1.
[0059] (3) 100 parts of polytetramethylene glycol were heated to 105° C. with stirring, dehydrated for 7 h, released from vacuum, cooled to below 50° C., then 250 parts of methylcyclohexyl diisocyanate were added and reacted at 100° C. for 4 h, 10 parts of intermediate product 2 were added and stirred for 6 h to obtain component A;
[0060] (4) 60 parts of trifunctional amino-terminated polyether, 50 parts of polyester diol, 2 parts of coupling agent phosphate coupling agent, 40 parts of 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane, 1 part of tetrabutyl borate, 5 parts of molecular sieve with specification 4a and 5 parts of color paste are stirred, ground and filtered to obtain component B;
[0061] (5) Component A and component B are mixed in a volume ratio of 1:1 to obtain an explosion-proof polyurea material.
[0062] Embodiment 3:
[0063] (1) 0.5 parts of nano-aramid fiber was added to 200 parts of 50% sodium dichloroisocyanurate aqueous solution, and dispersed and mixed at a speed of 2500 r / min for 6 minutes. After filtering to remove water, the mixture was reacted in an oven at 60° C. for 3 hours. After adding hydrochloric acid solution, the mixture was heated at 110° C. for 1.5 hours. The product was washed with deionized water and finally dried in an oven at 100° C. for 7 hours to obtain modified aramid fiber;
[0064] (2) 1.5 parts of modified aramid fiber, 30 parts of hexamethylene diisocyanate and 0.04 parts of tetraisopropyl borate were mixed and stirred for ultrasonic reaction in a closed nitrogen environment at room temperature for 10 hours. After the reaction, the residual HDI on the surface was cleaned with hexane to ensure that the solvent on the surface of the aramid fiber was cleaned. Finally, the fiber was dried at 55°C for use to obtain an intermediate product 1.
[0065] (3) 60 parts of polycaprolactone diol were heated to 100° C. with stirring, dehydrated for 6 hours, released from vacuum, cooled to below 50° C., then 200 parts of xylene diisocyanate were added and reacted at 90° C. for 3.5 hours, 6 parts of intermediate product 1 were added and stirred for 5 hours to obtain component A;
[0066] (4) 20 parts of difunctional amino-terminated polyether and 30 parts of trifunctional amino-terminated polyether, 30 parts of polyoxypropylene glycol, 10 parts of polycaprolactone glycol, 1.5 parts of borate coupling agent, 30 parts of 2,4-diamino-3-methylthio-5-propyltoluene, 0.6 parts of catalyst triethylenediamine, 2 parts of molecular sieve with specification 4a and 2 parts of color paste are stirred, ground and filtered to obtain component B;
[0067] (5) Component A and component B are mixed in a volume ratio of 1:1 to obtain an explosion-proof polyurea material.
[0068] Comparative Example 1:
[0069] (1) adding 0.5 parts of nano-aramid fiber to 200 parts of 50% hypochlorous acid aqueous solution, dispersing and mixing at a speed of 2500 r / min for 6 min, filtering to remove water, reacting in an oven at 60° C. for 3 hours, adding hydrochloric acid solution, heating at 110° C. for 1.5 hours, washing the product with deionized water, and finally drying in an oven at 100° C. for 7 hours to obtain modified aramid fiber;
[0070] (2) 1.5 parts of modified aramid fiber, 30 parts of hexamethylene diisocyanate and 0.04 parts of tetraisopropyl borate were mixed and stirred for ultrasonic reaction in a closed nitrogen environment at room temperature for 10 hours. After the reaction, the residual HDI on the surface was cleaned with hexane to ensure that the solvent on the surface of the aramid fiber was cleaned. Finally, the fiber was dried at 55°C for use to obtain an intermediate product 1.
[0071] (3) 60 parts of polycaprolactone diol were heated to 100° C. with stirring, dehydrated for 6 hours, released from vacuum, cooled to below 50° C., then 200 parts of polyisocyanate xylylene diisocyanate were added and reacted at 90° C. for 3.5 hours, 6 parts of intermediate product 1 were added and stirred for 5 hours to obtain component A;
[0072] (4) 20 parts of difunctional amino-terminated polyether and 30 parts of trifunctional amino-terminated polyether, 30 parts of polyoxypropylene glycol, 10 parts of polycaprolactone glycol, 1.5 parts of borate coupling agent, 30 parts of 2,4-diamino-3-methylthio-5-propyltoluene, 0.6 parts of catalyst triethylenediamine, 2 parts of molecular sieve with specification 4a and 2 parts of color paste are stirred, ground and filtered to obtain component B;
[0073] (5) Component A and component B are mixed in a volume ratio of 1:1 to obtain an explosion-proof polyurea material.
[0074] Comparative Example 2:
[0075] (1) 0.5 parts of nano-aramid fiber was added to 200 parts of 50% sodium dichloroisocyanurate aqueous solution, and dispersed and mixed at a speed of 2500 r / min for 6 minutes. After filtering to remove water, the mixture was reacted in an oven at 60° C. for 3 hours. After adding hydrochloric acid solution, the mixture was heated at 110° C. for 1.5 hours. The product was washed with deionized water and finally dried in an oven at 100° C. for 7 hours to obtain modified aramid fiber;
[0076] (2) 1.5 parts of modified aramid fiber, 30 parts of diphenylmethane-4,4'-diisocyanate and 0.04 parts of tetraisopropyl borate were mixed and stirred for ultrasonic reaction in a closed nitrogen environment at room temperature for 10 hours. After the reaction, the residual HDI on the surface was cleaned with hexane to ensure that the solvent on the surface of the aramid fiber was cleaned. Finally, the fiber was dried at 55°C for use to obtain an intermediate product 1.
[0077] (3) 60 parts of polycaprolactone diol were heated to 100° C. with stirring, dehydrated for 6 hours, released from vacuum, cooled to below 50° C., then 200 parts of polyisocyanate xylylene diisocyanate were added and reacted at 90° C. for 3.5 hours, 6 parts of intermediate product 1 were added and stirred for 5 hours to obtain component A;
[0078] (4) 20 parts of difunctional amino-terminated polyether and 30 parts of trifunctional amino-terminated polyether), 30 parts of polyoxypropylene glycol, 10 parts of polycaprolactone diol, 1.5 parts of borate coupling agent, 30 parts of 2,4-diamino-3-methylthio-5-propyltoluene (TX-3), 0.6 parts of triethylenediamine, 2 parts of molecular sieve with specification 4a and 2 parts of color paste are stirred, ground and filtered to obtain component B;
[0079] (5) Component A and component B are mixed in a volume ratio of 1:1 to obtain an explosion-proof polyurea material.
[0080] Comparative Example 3:
[0081] (1) 1.5 parts of nano-aramid fiber, 30 parts of hexamethylene diisocyanate and 0.04 parts of tetraisopropyl borate were mixed, stirred and ultrasonically reacted in a closed nitrogen environment at room temperature for 10 hours. After the reaction, the residual HDI on the surface was cleaned with hexane to ensure that the solvent on the surface of the aramid fiber was cleaned, and finally dried at 55°C for use to obtain an intermediate product.
[0082] (2) 60 parts of polycaprolactone diol were heated to 100° C. with stirring, dehydrated for 6 hours, released from vacuum, cooled to below 50° C., then 200 parts of xylene diisocyanate were added and reacted at 90° C. for 3.5 hours, 6 parts of the intermediate product were added and stirred for 5 hours to obtain component A;
[0083] (3) 20 parts of difunctional amino-terminated polyether and 30 parts of trifunctional amino-terminated polyether, 30 parts of polyoxypropylene glycol, 10 parts of polycaprolactone glycol, 1.5 parts of borate coupling agent, 30 parts of 2,4-diamino-3-methylthio-5-propyltoluene, 0.6 parts of catalyst triethylenediamine, 2 parts of molecular sieve with specification 4a and 2 parts of color paste are stirred, ground and filtered to obtain component B;
[0084] (4) Component A and component B are mixed in a volume ratio of 1:1 to obtain an explosion-proof polyurea material.
[0085] The components A and B prepared in Examples 1-3 and Comparative Examples 1-3 were mixed evenly by a sprayer and sprayed on the surface of the steel plate at a spraying pressure of 10 MPa and a spraying temperature of 65°C. The coating was placed in an environment with a temperature of (25±2)°C and a humidity of (50±5)%. After curing for 7 days, performance tests were performed. The results are shown in Table 1:
[0086] Table 1 Test results
[0087]
[0088] From the comparison between Examples 1-3 and Comparative Example 1, it can be seen that the tensile strength of Examples 1-3 is about 50% higher than that of Comparative Example 1, the elongation at break is about 10% higher than that of Comparative Example 1, and the tear strength is about 30% higher than that of Comparative Example 1, indicating that the use of sodium dichloroisocyanurate in the modified aramid fiber in the present invention has a great influence on the tensile strength, elongation at break and tear strength of the polyurea material, and the gun blocking occurs in Comparative Example 1, which also indicates that sodium dichloroisocyanurate has an influence on the spraying construction of the polyurea material of the present application.
[0089] From the comparison between Examples 1-3 and Comparative Example 2, it can be seen that the tensile strength of Examples 1-3 is about 80% higher than that of Comparative Example 2, the elongation at break is about 7% higher, and the tear strength is about 1 times higher, but the spraying construction effect is basically the same as that of Examples 1-3.
[0090] From the comparison between Examples 1-3 and Comparative Example 3, it can be seen that the tensile strength of Examples 1-3 is about 1 times higher than that of Comparative Example 3, the tear strength is about 1 times higher than that of Comparative Example 3, the elongation at break is about 5% higher than that of Comparative Example 3, and the gun is blocked in Comparative Example 3. This indicates that the chemical modification of aramid to prepare the intermediate product 1 in the process of preparing polyurea in the present invention has a great influence on the tensile strength and tear strength of the polyurea material of the present invention, and affects the spraying construction effect.
[0091] Although embodiments of the present invention have been shown and described (see the above detailed description for details), it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to these embodiments without departing from the principles and spirit of the present invention, and the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. An explosion-proof polyurea material, It is characterized in that The raw materials for preparing the polyurea material include component A and component B. The raw materials of component A include chlorine-activated modified aramid fiber with amino and carboxyl groups.
2. The explosion-proof polyurea material according to claim 1, wherein the structural formula of the modified aramid fiber is:
3. The explosion-proof polyurea material according to claim 1, wherein the raw materials of component A further include hexamethylene diisocyanate, a catalyst, a polyol and a polyisocyanate; The raw materials of the modified aramid fiber include nano-aramid fiber and sodium dichloroisocyanurate.
4. The explosion-proof polyurea material according to claim 1, Features: The preparation steps of the A component include: (1) adding an appropriate amount of nano-aramid fiber to an appropriate amount of sodium dichloroisocyanurate aqueous solution, adding an appropriate amount of hydrochloric acid after the reaction is completed, heating, purifying and drying to obtain the modified aramid fiber; (2) An appropriate amount of modified aramid fiber, hexamethylene diisocyanate and a catalyst are mixed, and after the reaction is completed, the mixture is purified and dried to obtain an intermediate product 1, wherein the intermediate product 1 has the structural formula: (3) Pre-treating the polyol, then adding a proper amount of polyisocyanate, and after the reaction is completed, adding a proper amount of intermediate product 1 to obtain component A.
5. The explosion-proof polyurea material according to claim 4, It is characterized in that The mass ratio of the nano-aramid fiber to the sodium dichloroisocyanurate aqueous solution is 0.1-1:250-350 parts, and the concentration of the sodium dichloroisocyanurate aqueous solution is 50%; The mass ratio of the modified aramid fiber, hexamethylene diisocyanate and catalyst is 1-2:25-35:0-0.1; The mass ratio of the polyol, the polyisocyanate and the intermediate product 1 is 50-100:150-250:200-350.
6. The explosion-proof polyurea material according to claim 4, Features: The process conditions of step (1) are as follows: the nano-aramid fiber is added to the sodium dichloroisocyanurate aqueous solution and dispersed and mixed at a speed of 2000-3000 r / min for 2-8 minutes, the water is filtered off and then reacted in an oven at 50-80° C. for 1-5 hours, the hydrochloric acid solution is added and then heated at 100-120° C. for 1-2 hours, the product is washed with deionized water, and finally dried in an oven at 90-110° C. for 6-8 hours; The process conditions of step (2) are as follows: stirring the ultrasonic reaction in a closed nitrogen environment at room temperature for 8-15 hours, washing the residual HDI on the surface with hexane after the reaction to ensure that the solvent on the surface of the nano-aramid fiber is cleaned, and finally drying at 50-60° C. for standby use; The pretreatment process conditions of step (3) are to heat the polyol to 95-105°C with stirring, dehydrate for 5-7h, release the vacuum, and cool to below 50°C; the reaction process conditions are to add the polyisocyanate, react at 80-100°C for 3-4h, and then add the intermediate 1 and continue stirring for 4-6h.
7. The explosion-proof polyurea material according to claim 3, Features: The purity of the nano-aramid fiber is ≥99% and the specific surface area is 7-11m 2 / g.
8. The explosion-proof polyurea material according to claim 3, Features: The -NCO content of the isocyanate prepolymer of the A component is 14% to 17%; the isocyanate index of the A component and the B component is 1.05 to 1.
10.
9. The explosion-proof polyurea material according to claim 3, Features: The polyisocyanate is one or more of diphenylmethane diisocyanate, isophorone diisocyanate, dicyclohexylmethane diisocyanate, methylcyclohexyl diisocyanate, cyclohexane dimethylene diisocyanate, xylylene diisocyanate, and 1,4-cyclohexane diisocyanate; The catalyst comprises one or more of bismuth isooctanoate, zinc isooctanoate, triethylenediamine, bismorpholinyl diethyl ether, tetrabutyl borate, and tetraisopropyl borate; The raw materials of component B include: amino-terminated polyether, polyol, coupling agent, chain extender, catalyst, dehydrating agent and color paste; The amino-terminated polyether includes one or more of difunctional amino-terminated polyether and trifunctional amino-terminated polyether; The polyol is one or more of polyoxypropylene glycol, polytetramethylene glycol, polycaprolactone glycol, polyester glycol, and polycarbonate glycol, and the average molecular weight of the polyol is 400-1500, the water content is ≤0.5%, and the acid value is ≤0.8 mg KOH / g; The coupling agent is one or more of a silane coupling agent, a borate coupling agent, an aluminate coupling agent, a borate coupling agent, a bimetallic coupling agent, and a phosphate coupling agent; The dehydrating agent is a molecular sieve, and the specification of the molecular sieve is 3a or 4a; The chain extender includes 3,5-dimethylthiotoluenediamine (E-300), 2,4-diamino-3,5-dimethylthiochlorobenzene (TX-2), 4,4′-bis-sec-butylaminodiphenylmethane (Unilink4200), N,N,-dialkylphenylenediamine, 2,4-diamino-3-methylthio-5-propyltoluene (TX-3), 3,3′-dimethyl-4,4′-diaminodicyclohexylmethane, 4,4,-bis-sec-butylaminodicyclohexylmethane, 3,3,-dimethyl-4,4,-bis-sec-butylamino-dicyclohexylmethane, trimethylhexanediamine or hydrogenated MDA; The mass ratio of the amino-terminated polyether, polyol, coupling agent, chain extender, catalyst, water scavenger and color paste is 30-60:20-50:1-2:20-40:0-1:1-5:1-5.
10. A method for preparing an explosion-proof polyurea material, It is characterized in that The steps of the preparation method include: (1) adding an appropriate amount of nano-aramid fiber to an appropriate amount of sodium dichloroisocyanurate aqueous solution, adding hydrochloric acid after the reaction is completed, heating, purifying and drying to obtain modified aramid fiber; (2) mixing an appropriate amount of modified aramid fiber, hexamethylene diisocyanate and a catalyst, and after the reaction is completed, purifying and drying to obtain an intermediate product 1; (3) pre-treating the polyol, then adding an appropriate amount of polyisocyanate, and after the reaction is completed, adding an appropriate amount of intermediate product 1 to obtain component A; (4) mixing appropriate amounts of amino-terminated polyether, polyol, coupling agent, chain extender, catalyst, water scavenger and color paste to obtain component B; (5) Component A and component B are mixed to obtain an explosion-proof polyurea material.
Citation Information
Patent Citations
Anti-knock bulletproof coating material and preparation method and application thereof
CN108707415A
High-strength sound-insulation polyurethane urea composite material
CN112679941A
Polyurethane resin