Rare-earth-based temperature-sensitive organic supramolecular gel accelerated ice melting coating material and preparation method thereof
Through rare earth-based temperature-sensitive organic supramolecular gel materials, the endothermic effect of rare earth compounds and the hydrophobicity of quad-carbon bromine chain aromatic hydrocarbons are used to solve the problems of low railway deicing efficiency and high labor costs, and achieve rapid at low temperatures Melting ice and efficient deicing are suitable for areas prone to icing on high-speed trains.
Patent Information
- Application Number
- CN202410948352.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-07-16
AI Technical Summary
The existing railway deicing method has limitations on the use of external forces and extreme conditions for precision components, and the cost of manual deicing is high, and the wear of the vehicle body cannot be avoided. The deicing time of high-speed trains is long, and the deicing efficiency of existing materials at low temperatures is low. .
Using rare earth-based temperature-sensitive organic supramolecular gel to accelerate melt-ice coating material, the chemical bonding of tetracarbon bromine chain column aromatic hydrocarbons and rare earth nanoborides is combined with triazole cyano group modified alkyl compounds to form high transition temperatures and hydrophobic gels, using the endothermic effect of rare earth compounds to achieve rapid melting of ice.
It quickly melts the ice at lower temperatures, reduces manual deicing time, reduces body wear, improves deicing efficiency, and extends the service life of the coating. It is suitable for freezing parts of high-speed trains.
Smart Images

Figure CN118879202A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of railway deicing, and in particular relates to a rare earth-based temperature-sensitive organic supramolecular gel accelerated ice-melting coating material and a preparation method thereof. Background Art
[0002] The existing railway deicing method usually uses natural ice melting in warm storage and high temperature and high pressure to de-ice the car body. However, for some precision parts, large external forces and extreme conditions cannot be used to achieve de-icing. In addition, a high-speed train needs dozens of people to de-ice continuously for more than three or four hours. Frequent cold night operations also increase labor costs. In the process of manual de-icing, it is inevitable that the car body will be worn to varying degrees. Summary of the invention
[0003] In view of this, the present invention aims to propose a rare earth-based thermosensitive organic supramolecular gel accelerated ice-melting coating material and a preparation method, which not only prevents the train from icing during operation, but also allows the ice to melt quickly under the action of rare earth compounds by heating at a relatively low temperature (15-20°C).
[0004] To achieve the above object, the technical solution of the present invention is achieved as follows:
[0005] A rare earth-based temperature-sensitive organic supramolecular gel accelerated ice-melting coating material is prepared from raw materials including the following weight percentages: 59.81-63.47% of a main body, 29.91-49.95% of a guest, and 0.07-10.28% of a solvent; wherein the main body includes the following weight percentages of raw materials: 77%-84.66% of tetracarbon bromine chain aromatic hydrocarbons, 4.86%-13.47% of a rare earth nano boride, 3.3%-3.63% of a reaction solvent, 4.84%-5.32% of a catalyst, and 1.39%-1.53% of an auxiliary catalyst; the guest is an alkyl compound modified by a triazole cyanide group, and the rare earth nano boride is a rare earth boride with active hydroxyl groups on the surface.
[0006] The tetra-carbon bromine chain aromatic hydrocarbon not only has a large cavity that can interact with the guest through host-guest interactions, but also has a long alkyl chain that reduces its steric hindrance, enabling it to undergo a better substitution reaction with rare earth compounds.
[0007] The rare earth nano-boride is not added to the system in a mixed manner, but needs to react with tetrabromo-chain columnar aromatics according to a stoichiometric ratio, and the columnar aromatics are chemically bonded.
[0008] The transition temperature is affected by the physical properties of the obtained structure and is only affected by the structure. The increase in the transition temperature is due to the use of cyano groups in the guest that have a stronger bond to the pillararene cavity.
[0009] Furthermore, the rare earth nano-boride is one or more of lanthanum hexaboride, neodymium hexaboride, samarium hexaboride, and praseodymium hexaboride; preferably, the rare earth nano-boride is lanthanum hexaboride; and the particle size D50 of the rare earth nano-boride is less than 90 nm.
[0010] The rare earth compound is a rare earth compound with photothermal effect, wherein the rare earth compound is prepared in such a way that it has active hydroxyl groups on its surface. Such hydroxyl groups will undergo substitution reaction with bromine to connect the rare earth compound to the polymer chain. Its main function is to quickly heat up the polymer by absorbing heat to achieve the effect of melting ice and de-icing.
[0011] Furthermore, the reaction solvent is one or more of acetonitrile, tetrahydrofuran, and pyridine.
[0012] Furthermore, the catalyst is one or more of sodium carbonate and potassium carbonate.
[0013] Furthermore, the catalyst is potassium carbonate powder after anhydrous drying treatment.
[0014] These catalysts are conducive to the removal of halogen atoms in a weakly alkaline environment, thereby causing a substitution reaction. At the same time, the potassium carbonate here is preferably anhydrous and dried potassium carbonate powder so that it can absorb trace moisture in the reaction environment.
[0015] Furthermore, the auxiliary catalyst is one or more of potassium iodide and sodium tungstate.
[0016] The auxiliary catalyst is a co-catalyst in the reaction process, which assists potassium carbonate in activating the short carbon chain monomer sites with large steric hindrance to cause a substitution reaction.
[0017] Further, the four-carbon bromine chain aromatics are prepared by the following method:
[0018] a) using 1,4-dibromobutane and p-hydroxyphenol to react in acetonitrile under the catalysis of potassium carbonate and potassium iodide to obtain anisole modified with a four-carbon bromine chain;
[0019] b) The tetra-carbon bromine chain-modified anisole is used as a raw material to react with p-phenylenedimethyl ether and polyformaldehyde in dichloromethane in an ice bath under the catalysis of boron trifluoride ether to obtain the product.
[0020] Furthermore, the triazole cyano modified alkyl compound is prepared by the following method: 1,10-dibromodecane and triazole cyano tetracarbon modified hydroxyphenol are refluxed in acetonitrile at 85°C and then filtered and dried.
[0021] The present invention also provides a method for preparing the rare earth-based temperature-sensitive organic supramolecular gel accelerated ice-melting coating material as described above, the method comprising the following steps:
[0022] 1) Preparation of four-carbon bromine chain aromatics;
[0023] 2) Preparation of the main body: Put the rare earth compound, catalyst and auxiliary catalyst powder dissolved in the reaction solvent into a constant pressure dropping funnel and drip into the reaction system of step 1) within 10 minutes, heat under reflux and stir for 48-54 hours, and then phase separate to obtain the main body;
[0024] 3) preparing a guest triazole cyano-modified alkyl compound;
[0025] 4) The host and the guest are uniformly mixed by ultrasonication in dimethyl sulfoxide, and the mixture is placed in a 20-30°C environment to stabilize for 2-8 minutes. The vial is taken out and turned upside down. If the sol does not drip along the wall, it is considered that a gel is formed.
[0026] The present invention also provides an application of the rare earth-based temperature-sensitive organic supramolecular gel accelerated ice-melting coating material as described above, and the material is used for railway deicing.
[0027] Compared with the prior art, the rare earth-based temperature-sensitive organic supramolecular gel accelerated ice-melting coating material and preparation method described in the present invention have the following advantages:
[0028] (1) The rare earth-based thermosensitive organic supramolecular gel accelerated ice-melting coating material of the present invention can make the rare earth exert its heat absorption effect to achieve rapid ice melting effect as the temperature rises during the operation of the train. At the same time, due to the strong interaction between the subject and the object, the three-dimensional structure is arranged very tightly, so it can better achieve the hydrophobic effect; therefore, a sol-gel transition occurs with the change of temperature. This transition will cause the ice layer to break, and due to the hydrophobic effect of the material, it can achieve the effect of easy deicing. At the same time, this material can be better coated on the parts of the high-speed rail that are prone to ice formation without becoming brittle and cracking due to the low temperature.
[0029] (2) The rare earth-based thermosensitive organic supramolecular gel accelerated ice melting coating material described in the present invention uses a single-modified columnar aromatic hydrocarbon, which has better flexibility than multi-modified compounds and is easy to produce structural transformation. At the same time, the compound modified with four carbon chains has a higher yield than the compound modified with a longer carbon chain, and can undergo substitution reaction faster than the long carbon chain at room temperature and pressure. In addition, the advantages of thermosensitive polymers themselves not requiring initiators, high product purity, and mild reaction conditions are also utilized. The lanthanum hexaboride is simply and easily connected to the polymer chain in the form of a chemical bond using a one-step synthesis method, which makes up for the shortcomings of low strength and poor toughness of inorganic nanoparticles and weak weather resistance and stability of organic matter. At the same time, the cyanide compound with a strong binding force with the columnar aromatic hydrocarbon cavity is used to make lanthanum hexaboride not easy to fall off with the phase transition during the deicing process, thereby losing the photothermal effect. The present invention uses a scanning electron microscope to obtain the structure of the rare earth-based thermosensitive organic supramolecular gel. This loose and porous structure confirms the successful preparation of the rare earth-based thermosensitive supramolecular polymer network.
[0030] (3) The rare earth-based thermosensitive organic supramolecular gel accelerated ice melting coating material described in the present invention utilizes the reversibility of hydrogen bonding to achieve the reversible transformation of the rare earth-based thermosensitive supramolecular gel, thereby increasing the reusability of the material. Hydrogen bonding is a single-atom non-covalent bond that can form a linear or network structure between molecules. The weak force between hydrogen bonds can be easily broken with changes in temperature, solvent, competitive molecules, etc., but can also be easily reconnected with the restoration of external conditions. Therefore, the present invention utilizes hydrogen bonding to achieve the reversible transformation of the rare earth-based thermosensitive organic supramolecular gel composite coating.
[0031] (4) The four-carbon chain columnar aromatic hydrocarbons used in the rare earth-based thermosensitive organic supramolecular gel accelerated ice-melting coating material described in the present invention have a shorter carbon chain and are more rigid than traditional flexible polymers. In addition, the object selected for preparation is triazole cyano, which has a strong binding ability with columnar aromatic hydrocarbons, so that the rigidity is further enhanced. Therefore, for this rigid system, the gel transition temperature of the formed supramolecular gel is higher than that of the flexible system, which can exceed 40°C. When the coating temperature gradually increases with the endothermic effect of the rare earth boride, the ice layer gradually melts. If the gel transition temperature is reached, a structural transformation will occur, which will reduce the adhesion of the ice layer, which is conducive to the shedding of the ice layer. At the same time, the rare earth compounds connected by chemical bonds will not peel off as the number of uses increases. In addition, the gel transition temperature of the material described in the present invention is higher. If the ice layer has melted before the gel transition temperature is reached, the coating will not be damaged. The coating only uses the hydrophobic group of the end group to achieve ice melting and ice protection, and the service life is further increased. Therefore, the material described in the present invention is more conducive to ice melting.
[0032] (5) The rare earth-based thermosensitive organic supramolecular gel accelerated ice melting coating material of the present invention selects rare earth compounds with surface hydroxylation because rare earth without hydroxyl groups will not be chemically bonded to columnar aromatics when mixed. In this way, the rare earth will also have an effect, but the wear will be very serious, or it will be easily peeled off by external force and cannot be reused. The columnar aromatics gel alone in Comparative Example 1 will also have an anti-icing effect, but if it does not produce a synergistic effect with the rare earth, its transition temperature (28-32°C) will also change. This change is not conducive to the gel-sol transition because the transition temperature will become lower without adding rare earth, but it does not have an endothermic effect, so the transition time will be longer under the same environment. However, since rare earth can absorb heat, it can achieve rapid temperature rise, making the transition time very short, much shorter than the time without adding rare earth.
[0033] (6) The rare earth-based thermosensitive organic supramolecular gel accelerated ice melting coating material of the present invention selects rare earth hexaboride with LSPR effect. For ordinary rare earth oxides, the electromagnetic wave absorption peak caused by LSPR is located in the visible light region, while the free electron density of rare earth hexaboride is small, the absorption peak is located in the near infrared region, and it has good near infrared absorption performance. The reason for not selecting rare earth oxides is that they do not have LSPR effect and do not have excellent near infrared absorption performance. Therefore, rare earth oxides with almost no heat absorption effect cannot achieve the deicing function.
[0034] (7) The rare earth-based thermosensitive organic supramolecular gel accelerated ice-melting coating material described in the present invention utilizes the super strong binding force between triazole cyanide and the macrocyclic cavity of columnar aromatic hydrocarbon to enable it to undergo gel-sol transition at a higher temperature (40-45°C), which greatly increases the corrosion resistance of the coating. The introduction of rare earth base enables the material to heat up in a short time, accelerating the melting time of the ice layer. The porous hydrophobic nature of the material can prevent the ice layer from adhering to the coating. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] The accompanying drawings constituting a part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the accompanying drawings:
[0036] Figure 1 A schematic diagram of the structure of the rare earth-based temperature-sensitive organic supramolecular gel accelerated ice-melting coating material of the invention;
[0037] Figure 2 The figure is a synthetic route for the host and the alkyl compound modified with triazole cyano group; (a) is a flow chart for the preparation of the host; (b) is a flow chart for the preparation of the guest;
[0038] Figure 3 This is an electron microscope image of the rare earth-based temperature-sensitive organic supramolecular gel accelerated ice-melting coating material prepared in Example 1;
[0039] Figure 4 A multi-step synthesis process for preparing rare earth-free thermosensitive polymers;
[0040] Figure 5 The comparison ice melting curves of Example 1 and Comparative Example 1;
[0041] Figure 6 is the ice melting control curve of Example 2-4;
[0042] Figure 7 It is the ice melting comparison curve of Example 1 and Comparative Example 2. DETAILED DESCRIPTION
[0043] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other.
[0044] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0045] Example 1
[0046] The preparation method of the rare earth-based temperature-sensitive organic supramolecular gel accelerated ice-melting coating material is as follows:
[0047] 1) Preparation of four-carbon bromine chain aromatics
[0048] 1,4-Dibromobutane (2.16 g, 10.00 mmol) and p-hydroxyphenol (1.70 g, 10.00 mmol) were reacted in acetonitrile (35 mL) under the catalysis of potassium carbonate (0.30 g, 2.15 mmol) and potassium iodide (0.11 g, 0.65 mmol) to obtain tetracarbon bromine chain-modified anisole, which was then used as a raw material with p-phenylenedimethyl ether (11.04 g, 80.00 mmol) and polyformaldehyde (1.35 g, 15.00 mmol) under the catalysis of boron trifluoride ether (3 mL) in dichloromethane (80 mL) in an ice bath to obtain.
[0049] 2) Preparation of the main body
[0050] First, lanthanum hexaboride (0.37 g, 1.84 mmol, particle size D50 < 90 nm), a rare earth compound with active hydroxyl groups on the surface, potassium carbonate powder (0.40 g, 2.94 mmol) and potassium iodide powder (0.12 g, 0.70 mmol) were dissolved in acetonitrile (100 mL), and then added to a constant pressure dropping funnel and dropped into the solution system obtained in step 1) within 10 minutes. The tetracarbon bromine chain aromatic hydrocarbon in the system was 6.4 g and 7.36 mmol. The mixture was then heated to reflux and stirred for 48 hours. After the reaction was completed, the temperature was lowered and the solid was filtered out by a suction filtration device, and the filtrate in the suction flask was evaporated to remove the solvent by a rotary evaporator at 36°C.
[0051] The crude product was dissolved in dichloromethane (300 mL) and washed with water (140 mL) three times. After separation using a separatory funnel, anhydrous magnesium sulfate was added for drying, and then silica gel was added for spin drying. It was purified by column chromatography, wherein the eluent was petroleum ether and ethyl acetate in a volume ratio of 2:1, and finally the main product (0.72 g, yield 21%) was obtained in the form of a white powder.
[0052] 3) Preparation of triazole cyano-modified alkyl compounds (guests)
[0053] First, alkynylphenol (2.96 g, 20.00 mmol) and azide (2.48 g, 20.00 mmol) were heated to reflux in DMF (20 mL) under the catalysis of cuprous iodide (0.95 g, 5 mmol) for 12 hours, and the triazole-modified precursor was obtained after extraction and spin-drying. Then, the precursor modified with triazole cyano group (5.74 g, 20.00 mmol) was dissolved in a round-bottom flask with acetonitrile (30 mL), and then 1,10-dibromodecane (6.62 g, 22.05 mmol) and acetonitrile (80 mL) were mixed evenly in a dropping funnel and placed on top of the round-bottom flask. The solution was uniformly dropped into the flask with stirring and condensed under reflux at 85°C. After 12 hours, it was cooled to room temperature, and suspended solids were produced in the solution. Subsequently, the solid-liquid separation was carried out using a suction flask and a funnel and the solution was washed with acetonitrile. The solid was placed in a vacuum drying oven and dried at 60°C in vacuum overnight to obtain a light yellow triazole cyano group-modified alkyl compound (guest) product (8.40 g, yield 72%).
[0054] 4) The main body and the triazole cyano-modified alkyl compound were ultrasonically dissolved in 10 mL of dimethyl sulfoxide at 60° C. in a mass ratio of 92:17. After the system was uniform, it was allowed to stand and a gel was formed after 5 minutes.
[0055] The electron microscope image of the rare earth-based temperature-sensitive organic supramolecular gel accelerated ice melting coating material is shown in Figure 3 As shown, it can be seen from the figure that the material has a loose and porous structure.
[0056] Observation shows that the transition temperature of the rare earth-based thermosensitive organic supramolecular gel accelerated ice-melting coating material is 40-41°C.
[0057] In the freezer experiment, an iron plate coated with the material was placed in a freezer at -20°C for 24 hours, and the frozen coating did not crack.
[0058] Example 2
[0059] The preparation method of the rare earth-based temperature-sensitive organic supramolecular gel accelerated ice-melting coating material is as follows:
[0060] 1) Preparation of four-carbon bromine chain aromatics as in step 1 of Example 1).
[0061] 2) Preparation of the main body
[0062] First, lanthanum hexaboride (0.60 g, 2.94 mmol, particle size D50 < 90 nm), a rare earth compound with active hydroxyl groups on the surface, potassium carbonate powder (0.40 g, 2.94 mmol) and potassium iodide powder (0.12 g, 0.7 mmol) were dissolved in acetonitrile (100 mL), and then added to a constant pressure dropping funnel and dripped into the solution system obtained in step 1) within 10 minutes. The tetracarbon bromine chain aromatic hydrocarbon in the system was 6.4 g and 7.36 mmol. The mixture was then heated to reflux and stirred for 48 hours. The post-treatment was the same as the steps in Example 1, and finally the main product (1.65 g, yield 30%) in the form of a white powder was obtained.
[0063] 3) The preparation of the triazole cyano-modified alkyl compound (guest) is the same as step 3) in Example 1.
[0064] 4) The dimer and the triazole cyano-modified alkyl compound were ultrasonically dissolved in 10 mL of dimethyl sulfoxide at 60° C. in a ratio of 92:17, and the system was allowed to stand until it was uniform, and a gel was formed after 5 minutes.
[0065] Observation shows that the transition temperature of the rare earth-based thermosensitive organic supramolecular gel accelerated ice-melting coating material is 41-43°C.
[0066] In the freezer experiment, an iron plate coated with the material was placed in a freezer at -20°C for 24 hours, and the frozen coating did not crack.
[0067] Example 3
[0068] The preparation method of the rare earth-based temperature-sensitive organic supramolecular gel accelerated ice-melting coating material is as follows:
[0069] 1) Preparation of four-carbon bromine chain aromatics as in step 1 of Example 1).
[0070] 2) Preparation of the main body
[0071] First, lanthanum hexaboride (0.75 g, 3.68 mmol, particle size D50 < 90 nm), potassium carbonate powder (0.40 g, 2.94 mmol) and potassium iodide powder (0.12 g, 0.7 mmol) with active hydroxyl groups on the surface were dissolved in acetonitrile (100 mL), and then added to a constant pressure dropping funnel and dripped into the solution system obtained in step 1) within 10 min. The four-carbon bromine chain aromatic hydrocarbon in the system was 6.4 g and 7.36 mmol. The mixture was then heated and refluxed for 48 hours, and the post-treatment was the same as in Example 1. Finally, the main product (1.24 g, yield 18%) was obtained in the form of a white powder.
[0072] 3) The preparation of the triazole cyano-modified alkyl compound (guest) is the same as step 3) in Example 1.
[0073] 4) The dimer and the triazole cyano-modified alkyl compound were ultrasonically dissolved in 10 mL of dimethyl sulfoxide at 60° C. in a ratio of 92:17, and the system was allowed to stand until it was uniform, and a gel was formed after 5 minutes.
[0074] Observation shows that the transition temperature of the rare earth-based thermosensitive organic supramolecular gel accelerated ice-melting coating material is 43-45°C.
[0075] In the freezer experiment, an iron plate coated with the material was placed in a freezer at -20°C for 24 hours, and the frozen coating did not crack.
[0076] Example 4
[0077] The preparation method of the rare earth-based temperature-sensitive organic supramolecular gel accelerated ice-melting coating material is as follows:
[0078] 1) Preparation of four-carbon bromine chain aromatics as in step 1 of Example 1).
[0079] 2) Preparation of the main body
[0080] First, lanthanum hexaboride (1.12 g, 5.51 mmol, particle size D50 < 90 nm), potassium carbonate powder (0.40 g, 2.94 mmol) and potassium iodide powder (0.12 g, 0.7 mmol) with active hydroxyl groups on the surface were dissolved in acetonitrile (100 mL), and then added to a constant pressure dropping funnel and dripped into the solution system obtained in step 1) within 10 minutes. The four-carbon bromine chain aromatic hydrocarbon in the system was 3.2 g, 3.68 mmol. The mixture was then heated and refluxed for 48 hours, and the post-treatment was the same as in Example 1. Finally, the main product (0.82 g, yield 12%) was obtained in the form of a white powder.
[0081] 3) The preparation of the triazole cyano-modified alkyl compound (guest) is the same as step 3) in Example 1.
[0082] 4) The dimer and the triazole cyano-modified alkyl compound were ultrasonically dissolved in 10 mL of dimethyl sulfoxide at 60° C. in a ratio of 92:17, and the system was allowed to stand until it was uniform, and a gel was formed after 5 minutes.
[0083] Observation shows that the transition temperature of the rare earth-based thermosensitive organic supramolecular gel accelerated ice-melting coating material is 44-45°C.
[0084] In the freezer experiment, an iron plate coated with the material was placed in a freezer at -20°C for 24 hours, and the frozen coating did not crack.
[0085] Through Examples 1-4, it can be concluded that the transition temperature of the material prepared by the present invention is 40-45°C, which can prove that the material has good host-guest interaction, so that the material will not crack when frozen at -20°C in the freezer experiment, and the material has excellent toughness.
[0086] In Examples 1-4, the amount of rare earth is increased, and the transition temperature increases slightly, indicating that the rare earth can be embedded in the network structure of the gel after being combined with the single-modified columnar aromatic hydrocarbon in equal stoichiometric ratios. The non-covalent bond interaction can make the three-dimensional network structure of the gel tighter, thereby increasing the transition temperature. Compared with the original materials with equal stoichiometric ratios, the embedded rare earth has more heat-absorbing substances and has a better ice-melting effect.
[0087] In addition, through Figure 6 It can be seen that the ice melting rate gradually increases with the increase of rare earth addition.
[0088] Comparative Example 1
[0089] The preparation method of a multi-step synthetic rare earth-free temperature-sensitive polymer comprises the following steps:
[0090] 1) Four carbon modified four carbon chain aromatic hydrocarbon (2.00 g, 2.20 mmol) and potassium phthalimide (1.00 g, 5.00 mmol) were evaporated under vacuum, and the residue was purified by flash column chromatography on silica gel to give a yellow solid (2.00 g, 93%).
[0091] 2) The yellow solid (1.00 g, 1.06 mmol) and NH 2 NH 2 A mixture of 1% paraformaldehyde (10 mL) was heated to reflux in methanol (20 mL) for 12 h. The mixture was then filtered to give a white solid (0.51 g, 60%).
[0092] 3) DMAP and EDC (0.96 g, 5.00 mmol) were added to a solution of the white solid (2.00 g, 2.48 mmol) and 2,2'-bipyridine-4,4'-dicarboxylic acid (0.30 g, 1.23 mmol) in chloroform (50 mL), and the mixture was stirred at room temperature for 48 hours.
[0093] 4) The organic layer was washed with water and saturated NaHCO 3 Aqueous solution and brine washing, Na 2 SO 4 After drying and concentrating, the thermosensitive polymer can be purified by column chromatography.
[0094] It can be observed that the transition temperature of the rare earth-free thermosensitive polymer is 28-32°C.
[0095] In the freezer experiment, an iron plate coated with the material was placed in a freezer at -20°C for 24 hours, and the frozen coating did not crack.
[0096] In order to compare the difference between Example 1 and Comparative Example 1, the two materials were coated on the surface of the iron parts respectively, and water was dripped in a freezer at -20°C. When the weight of frozen ice reached 30g, the iron parts were transferred to a dry freezer and continued to freeze for 8h. Then, the iron parts were placed under the same light source for illumination, and the weight of ice within 20 minutes was recorded. The results are shown in FIG. Figure 5 As shown, it can be seen that the material with rare earth can achieve rapid ice melting and has completely melted in about 9 minutes. However, the material without rare earth still maintains about 18g of ice after 20 minutes, with almost no heat absorption and ice melting effect.
[0097] Comparative Example 2
[0098] The method for preparing rare earth oxide temperature-sensitive organic supramolecular gel comprises the following steps:
[0099] 1) Preparation of four-carbon bromine chain aromatics as in step 1 of Example 1).
[0100] 2) Preparation of the main body
[0101] First, cerium oxide (0.36 g, 2.1 mmol, particle size D50 < 90 nm), a rare earth compound with active hydroxyl groups on the surface, potassium carbonate powder (0.23 g, 1.68 mmol) and potassium iodide powder (0.066 g, 0.4 mmol) were dissolved in acetonitrile (100 mL), and then added to a constant pressure dropping funnel and dripped into the solution system obtained in step 1) within 10 minutes. The four-carbon bromine chain aromatic hydrocarbon in the system was 3.2 g and 3.68 mmol. The mixture was then heated and refluxed with stirring for 48 hours, and the post-treatment was the same as in Example 1. Finally, the main product in the form of a white powder can be obtained.
[0102] 3) The preparation of the triazole cyano-modified alkyl compound (guest) is the same as step 3) in Example 1.
[0103] 4) The dimer and the triazole cyano-modified alkyl compound were ultrasonically dissolved in 10 mL of dimethyl sulfoxide at 60° C. in a ratio of 92:17, and the system was allowed to stand until it was uniform, and a gel was formed after 5 minutes.
[0104] It can be found from observation that the transition temperature of the rare earth oxide thermosensitive polymer is 33-35°C.
[0105] In the freezer experiment, an iron plate coated with the material was placed in a freezer at -20°C for 24 hours, and the frozen coating did not crack.
[0106] In order to compare the difference between Example 1 and Comparative Example 2, the two materials were coated on the surface of the iron parts respectively, and water was dripped in a freezer at -20°C. When the weight of frozen ice reached 30g, the iron parts were transferred to a dry freezer and continued to freeze for 8h. Then, the iron parts were placed under the same light source for illumination, and the weight of ice within 20 minutes was recorded. The results are shown in FIG. Figure 7 As shown, it can be seen that since rare earth oxides do not have the LSPR effect of rare earth borides, even if they can be chemically bonded with the main body, they still cannot achieve excellent ice-melting effect.
[0107] This is because rare earth oxides do not have the LSPR effect and do not have excellent near-infrared absorption properties. Therefore, rare earth oxides, which have almost no heat absorption effect, cannot achieve the deicing function.
[0108] Comparative Example 3
[0109] The preparation method of the rare earth-based multi-chain modified organic supramolecular polymer material is as follows:
[0110] 1) Preparation of four-carbon bromine chain multi-modified column aromatics
[0111] 1,4-Dibromobutane (4.32 g, 20.00 mmol) and p-hydroxyphenol (1.70 g, 10.00 mmol) were reacted in acetonitrile (45 mL) under the catalysis of potassium carbonate (0.45 g, 3.23 mmol) and potassium iodide (0.11 g, 0.65 mmol) to obtain a four-carbon bromine chain multi-modified benzene ring compound, which was then used as a raw material and polyformaldehyde (1.35 g, 15.00 mmol) was reacted in dichloromethane (100 mL) in an ice bath under the catalysis of boron trifluoride ether (5 mL).
[0112] 2) Preparation of the main body
[0113] First, lanthanum hexaboride (0.66 g, 3.27 mmol), a rare earth compound with active hydroxyl groups on the surface, potassium carbonate powder (0.40 g, 2.94 mmol) and potassium iodide powder (0.12 g, 0.7 mmol) were dissolved in acetonitrile (100 mL), and then added to a constant pressure dropping funnel and dripped into the solution system obtained in step 1) within 10 minutes. The four-carbon bromine chain aromatic hydrocarbon in the system was 6.4 g and 3.27 mmol. The mixture was then heated and refluxed for 48 hours, and the post-treatment was the same as in Example 1. Finally, the main product (0.69 g, yield 10%) was obtained in the form of a white powder.
[0114] 3) The preparation of the triazole cyano-modified alkyl compound (guest) is the same as step 3) in Example 1.
[0115] 4) The main body and the triazole cyano-modified alkyl compound were ultrasonically dissolved in 10 mL of dimethyl sulfoxide at 60°C in a ratio of 92:17, and then cooled without gel formation. In addition, during the ice melting experiment after coating, the coating was easy to fall off because no three-dimensional network structure was formed.
[0116] It shows that the coating material modified with four-carbon chain columnar aromatics is more conducive to ice melting than the multi-chain modified one because the carbon chain is shorter and the rigidity is greater. In addition, the prepared guest is triazole cyanide, which has a strong binding ability with columnar aromatics, which further enhances the rigidity. Therefore, for this rigid system, the gel transition temperature of the formed supramolecular gel is higher than that of the flexible system, and can exceed 40°C.
[0117] Comparative Example 4
[0118] The method for preparing the temperature-sensitive organic supramolecular gel accelerated ice-melting coating material having a rare earth compound and no active hydroxyl groups on the surface is as follows:
[0119] 1) Preparation of four-carbon bromine chain aromatics
[0120] 1,4-Dibromobutane (2.16 g, 10.00 mmol) and p-hydroxyphenol (1.70 g, 10.00 mmol) were reacted in acetonitrile (35 mL) under the catalysis of potassium carbonate (0.30 g, 2.15 mmol) and potassium iodide (0.11 g, 0.65 mmol) to obtain tetracarbon bromine chain-modified anisole, which was then used as a raw material with p-phenylenedimethyl ether (11.04 g, 80.00 mmol) and polyformaldehyde (1.35 g, 15.00 mmol) under the catalysis of boron trifluoride ether (3 mL) in dichloromethane (80 mL) in an ice bath to obtain.
[0121] 2) Preparation of the main body
[0122] First, lanthanum hexaboride (0.37 g, 1.84 mmol, particle size D50 < 90 nm), a rare earth compound without active hydroxyl groups on the surface, potassium carbonate powder (0.40 g, 2.94 mmol) and potassium iodide powder (0.12 g, 0.70 mmol) were dissolved in acetonitrile (100 mL), and then added to a constant pressure dropping funnel and dropped into the solution system obtained in step 1) within 10 minutes. The four-carbon bromo-chain aromatic hydrocarbon in the system was 6.4 g and 7.36 mmol. The mixture was then heated to reflux and stirred for 48 hours. After the reaction was completed, the temperature was lowered and the solid was filtered out by a suction filtration device, and the filtrate in the suction flask was evaporated to remove the solvent by a rotary evaporator at 36°C.
[0123] The crude product was dissolved in dichloromethane (300 mL) and washed with water (140 mL) three times. After separation using a separatory funnel, anhydrous magnesium sulfate was added for drying, and then silica gel was added for spin drying, and it was purified by column chromatography, wherein the eluent was petroleum ether and ethyl acetate, and the volume ratio was 2:1. Since there was no hydroxyl group on the surface of lanthanum hexaboride and there was no site for binding with tetrabromo-chain aromatic hydrocarbons, the obtained substance was a physical mixture of tetrabromo-chain aromatic hydrocarbons and lanthanum hexaboride.
[0124] 3) Preparation of triazole cyano-modified alkyl compounds (guests)
[0125] First, alkynylphenol (2.96 g, 20.00 mmol) and azide (2.48 g, 20.00 mmol) were heated to reflux in DMF (20 mL) under the catalysis of cuprous iodide (0.95 g, 5 mmol) for 12 hours, and the triazole-modified precursor was obtained after extraction and spin-drying. Then, the precursor modified with triazole cyano group (5.74 g, 20.00 mmol) was dissolved in a round-bottom flask with acetonitrile (30 mL), and then 1,10-dibromodecane (6.62 g, 22.05 mmol) and acetonitrile (80 mL) were mixed evenly in a dropping funnel and placed on top of the round-bottom flask. The solution was uniformly dropped into the flask with stirring and condensed under reflux at 85°C. After 12 hours, it was cooled to room temperature, and suspended solids were produced in the solution. Subsequently, the solid-liquid separation was carried out using a suction flask and a funnel and the solution was washed with acetonitrile. The solid was placed in a vacuum drying oven and dried at 60°C in vacuum overnight to obtain a light yellow triazole cyano group-modified alkyl compound (guest) product (8.40 g, yield 72%).
[0126] 4) The main body and the triazole cyano-modified alkyl compound were ultrasonically dissolved in 10 mL of dimethyl sulfoxide at 60°C in a ratio of 92:17, and no gel was formed after cooling. In addition, during the ice melting experiment after coating, the coating was easy to fall off because no three-dimensional network structure was formed; at the same time, lanthanum hexaboride could not be embedded in the three-dimensional network, so it could not be mixed into the system and had no ice melting effect.
[0127] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A rare earth-based temperature-sensitive organic supramolecular gel accelerated ice-melting coating material, characterized in that: The material is prepared from raw materials including the following weight percentages: 59.81-63.47% of a main body, 29.91-49.95% of a guest, and 0.07-10.28% of a solvent; wherein the main body includes the following weight percentages of raw materials: 77%-84.66% of tetracarbon bromine chain aromatic hydrocarbons, 4.86%-13.47% of rare earth nano-borides, 3.3%-3.63% of a reaction solvent, 4.84%-5.32% of a catalyst, and 1.39%-1.53% of an auxiliary catalyst; the guest is an alkyl compound modified by a triazole cyanide group, and the rare earth nano-boride is a rare earth boride with active hydroxyl groups on the surface.
2. The rare earth-based temperature-sensitive organic supramolecular gel accelerated ice-melting coating material according to claim 1, characterized in that: The rare earth nano-boride is one or more of lanthanum hexaboride, neodymium hexaboride, samarium hexaboride and praseodymium hexaboride; preferably, the rare earth nano-boride is lanthanum hexaboride; and the particle size D50 of the rare earth nano-boride is less than 90 nm.
3. The rare earth-based temperature-sensitive organic supramolecular gel accelerated ice-melting coating material according to claim 1, characterized in that: The solvent in the raw material of the ice-melting coating material is one or more of dimethyl sulfoxide, DM, and acetonitrile; the main reaction solvent is one or more of acetonitrile, tetrahydrofuran, and pyridine.
4. The rare earth-based temperature-sensitive organic supramolecular gel accelerated ice-melting coating material according to claim 1, characterized in that: The catalyst is one or more of sodium carbonate and potassium carbonate.
5. The rare earth-based temperature-sensitive organic supramolecular gel accelerated ice-melting coating material according to claim 4, characterized in that: The catalyst is potassium carbonate powder after anhydrous drying.
6. The rare earth-based temperature-sensitive organic supramolecular gel accelerated ice-melting coating material according to claim 1, characterized in that: The auxiliary catalyst is one or more of potassium iodide and sodium tungstate.
7. The rare earth-based temperature-sensitive organic supramolecular gel accelerated ice-melting coating material according to claim 1, characterized in that: Four carbon bromine chain aromatics are prepared by the following method: a) using 1,4-dibromobutane and p-hydroxyphenol to react in acetonitrile under the catalysis of potassium carbonate and potassium iodide to obtain anisole modified with a four-carbon bromine chain; b) Anisole modified with a tetra-carbon bromine chain is used as a raw material to react with p-phenylenedimethyl ether and polyformaldehyde in dichloromethane in an ice bath under the catalysis of boron trifluoride ether to obtain the product.
8. The rare earth-based temperature-sensitive organic supramolecular gel accelerated ice-melting coating material according to claim 1, characterized in that: The triazole cyano modified alkyl compound is prepared by the following method: 1,10-dibromodecane and triazole cyano tetracarbon modified hydroxyphenol are refluxed in acetonitrile at 85° C. and then filtered and dried.
9. A method for preparing a rare earth-based temperature-sensitive organic supramolecular gel accelerated ice-melting coating material as claimed in any one of claims 1 to 8, characterized in that: The method comprises the following steps: 1) Preparation of four-carbon bromine chain aromatics; 2) Preparation of the main body: Put the rare earth compound, catalyst and auxiliary catalyst powder dissolved in the reaction solvent into a constant pressure dropping funnel and drip into the reaction system of step 1) within 10 minutes, heat under reflux and stir for 48-54 hours, and then phase separate to obtain the main body; 3) preparing a guest triazole cyano-modified alkyl compound; 4) The host and the guest are uniformly mixed by ultrasonication in dimethyl sulfoxide, and the mixture is placed in a 20-30°C environment to stabilize for 2-8 minutes. The vial is taken out and turned upside down. If the sol does not drip along the wall, it is considered that a gel is formed.
10. An application of the rare earth-based temperature-sensitive organic supramolecular gel accelerated ice-melting coating material as claimed in any one of claims 1 to 8, characterized in that: This material is used for railway deicing.
Citation Information
Patent Citations
Preparation method of supramolecular copolymerization column five-aromatic hydrocarbon gel
CN104826562A
Polymer, composition and coating and product thereof
CN113698535A
Two-component aqueous coating and coating layer with wear-resistance, low ice adhesiveness and Anti-icing, and preparation method and use thereof
WO2015100753A1