Shield foaming agent, preparation method thereof and method for improving characteristics of shield muck
Through the preparation of dry powder shield foam agent, biodegradable materials are used to improve the foaming multiple and stability, the problems of high transportation costs and environmental pollution of existing foam agents are solved, and efficient and environmentally friendly construction results are achieved.
Patent Information
- Application Number
- CN202411173822.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-01
AI Technical Summary
The existing shield foaming agent has insufficient foaming ratio, is difficult to degrade, and has high transportation costs, which affects construction efficiency and environment.
Dry powder shield foam agent, containing foaming agent, foam stabilizer, pH adjuster and foam lubricant, is prepared by mixing dry powder and water, to improve the foaming ratio and stability, and to utilize biodegradable materials Reduce environmental pollution.
It significantly improves the stability and durability of foam, reduces transportation costs, enhances construction efficiency, and is easy to degrade and reduces environmental pollution.
Smart Images

Figure BDA0005010130150000021 
Figure BDA0005010130150000111 
Figure BDA0005010130150000121
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of building construction, and in particular to a shield foaming agent and a preparation method thereof, and a method for improving the properties of shield slag. Background Art
[0002] In shield tunnel construction, a large amount of mud and slag will be excavated during the tunneling process of the shield machine. How to improve the characteristics of the slag and efficiently transport the slag has always been a problem to be solved in shield engineering. Foaming agents are widely used in soil improvement, and they are effective in reducing the cohesive friction of shield slag and improving tunneling efficiency. The specific use of the foaming agent is: injecting pressurized and aerated dense foam into the front of the shield machine cutter head, and under the action of the rotation of the cutter head, it is mixed with the cut slag to improve its performance, make the slag have plastic flow, and conveniently and quickly transport the slag.
[0003] The existing foaming agents have insufficient foaming multiples, resulting in insufficient and insufficiently dense foam; and most of them are inorganic chemical polymers, which are difficult to degrade after use, causing serious pollution and damage to soil and water quality, and adding huge impact and burden to subsequent restoration; and because most of the foaming agents on the market are liquid, the quantity shipped on one truck is limited, the transportation cost is greatly increased, and the transportation efficiency is not high. Summary of the invention
[0004] The purpose of the present application is to provide a shield foaming agent and a preparation method thereof, and a method for improving the properties of shield slag, aiming to solve the problems of insufficient foaming multiples, difficulty in degradation, and high transportation costs of existing foaming agents.
[0005] To achieve the above objectives, the present application provides a shield foaming agent, the shield foaming agent comprising dry powder and water, the dry powder comprising, by mass percentage:
[0006]
[0007] The mass ratio of the dry powder to the water is 1:15-25.
[0008] In some embodiments, the foaming agent is selected from sodium dodecylbenzene sulfonate and / or sodium lauryl sulfate.
[0009] In some embodiments, the foaming aid is tea saponin.
[0010] In some embodiments, the foam stabilizer is selected from coconut oil fatty acid diethanolamide.
[0011] In some embodiments, the pH adjuster is at least one of lactic acid and malic acid.
[0012] In some embodiments, the foam lubricant is selected from alkyl glycosides.
[0013] In some embodiments, the shield foaming agent has a foaming multiple of 20-30 and a foam half-life of 15-20 minutes.
[0014] The present application also provides a method for preparing the above-mentioned shield foaming agent, comprising:
[0015] A foaming agent, a foaming aid, a foam stabilizer, a pH regulator and a foam lubricant are mixed to obtain a dry powder shield foaming agent, and the dry powder shield foaming agent is mixed with water to obtain the shield foaming agent.
[0016] In some embodiments, the mixing time is 10-30 min, and the stirring speed is 800-1500 r / min.
[0017] The present application also provides a method for improving the properties of shield tunneling slag, using the above-mentioned shield tunneling foaming agent during the shield tunneling process.
[0018] Compared with the prior art, the beneficial effects of this application include:
[0019] The shield foam agent provided in the present application includes dry powder and water. Water can be added when in use. The dry powder includes a foaming agent, a foaming aid, a foam stabilizer, a pH adjuster and a foam lubricant. The dry powder can save a lot of transportation costs and improve transportation efficiency. For example, one truck can be loaded with 32 tons of liquid foam agent. 32 tons of powder can be diluted into 640 tons of liquid foam agent at a ratio of 1:19, and the difference in transportation costs is huge.
[0020] The raw materials selected above include anionic and nonionic components. Under the synergistic effect of multiple ionic components, the gaps between the foams become smaller, which significantly improves the stability and durability of the foam. Tea saponin, as a foaming aid, has a significant foaming and stabilizing effect. Since it is mostly plant extracts, its biodegradability can reach more than 95%, and it is suitable for various soil conditions and environments. The pH regulator regulates the pH value of the foaming agent and can effectively increase the adaptability of the foaming agent to different soil layers. The foam lubricant increases the wettability and plastic flow of the foam, making it easier to discharge the foam after entraining the slag. The interaction of various materials makes the foaming agent achieve excellent performance. The remaining materials are all easily degradable raw materials, with little pollution to the environment, high degradation rate, and green environmental protection. It has broad application prospects while effectively improving the quality and efficiency of shield tunnel construction. DETAILED DESCRIPTION
[0021] As used herein:
[0022] "Prepared from" is synonymous with "comprising." As used herein, the terms "comprising," "including," "having," "containing," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.
[0023] The conjunction "consisting of excludes any unspecified element, step, or component. If used in a claim, this phrase renders the claim closed-ended so that it does not include materials other than those described, except for conventional impurities associated therewith. When the phrase "consisting of" appears in a clause of the body of a claim rather than immediately following the subject matter, it limits only the elements described in that clause; other elements are not excluded from the claim as a whole.
[0024] When an amount, concentration, or other value or parameter is expressed as a range, a preferred range, or a range defined by a series of upper preferred values and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value with any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when a range of "1 to 5" is disclosed, the described range should be interpreted as including ranges "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5", etc. When a numerical range is described in this article, unless otherwise stated, the range is intended to include its end values and all integers and fractions within the range.
[0025] In these examples, parts and percentages are by mass unless otherwise indicated.
[0026] "Parts by mass" refers to the basic unit of measurement for expressing the mass ratio of multiple components. 1 part can represent any unit mass, such as 1g or 2.689g. If we say that the mass of component A is a parts and the mass of component B is b parts, it means the ratio of the mass of component A to the mass of component B is a:b. Alternatively, it means that the mass of component A is aK and the mass of component B is bK (K is an arbitrary number, indicating a multiple factor). It should not be misunderstood that, unlike the mass parts, the sum of the mass of all components is not limited to 100 parts.
[0027] "And / or" is used to indicate that one or both of the stated situations may occur, for example, A and / or B includes (A and B) and (A or B).
[0028] The present application provides a shield foaming agent, which includes dry powder and water. The dry powder, calculated by mass percentage, includes: 55%-65% of a foaming agent, 15%-20% of a foaming aid, 19%-25% of a foam stabilizer, 1%-2% of a pH adjuster, and 2%-5% of a foam lubricant; the mass ratio of the dry powder to the water is 1:15-25.
[0029] In some embodiments, the mass percentage of the foaming agent can be, for example, 55%, 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64%, 65% or any value between 55% and 65%; the foaming agent is selected from sodium dodecylbenzene sulfonate and / or sodium lauryl sulfate.
[0030] In some embodiments, the mass percentage of the foaming aid can be, for example, 15%, 16%, 17%, 18%, 19%, 20% or any value between 15% and 20%; the foaming aid is camellia seed extract - tea saponin.
[0031] In some embodiments, the mass percentage of the foam stabilizer can be, for example, 19%, 20%, 21%, 22%, 23%, 24%, 25% or any value between 19% and 25%; the foam stabilizer is selected from coconut oil fatty acid diethanolamide.
[0032] In some embodiments, the mass percentage of the pH adjuster may be, for example, 1%, 1.5%, 2%, or any value between 1% and 2%, and the pH adjuster may be at least one of lactic acid and malic acid.
[0033] In some embodiments, the mass percentage of the foam lubricant can be, for example, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5% or any value between 2% and 5%, and the foam lubricant is alkyl glycoside.
[0034] In some embodiments, the mass ratio of the dry powder to the water can be, for example, 1:15, 1:16, 1:17, 1:18, 1:19, 1:20, 1:21, 1:22, 1:23, 1:24, or 1:25.
[0035] In some embodiments, the shield foaming agent has a foaming multiple of 20-30 and a foam half-life of 15-20 minutes.
[0036] The present application also provides a method for preparing the above-mentioned shield foaming agent, comprising:
[0037] A foaming agent, a foaming aid, a foam stabilizer, a pH regulator and a foam lubricant are mixed to obtain a dry powder shield foaming agent, and the dry powder shield foaming agent is mixed with water to obtain the shield foaming agent.
[0038] In some embodiments, the mixing time is 10-30 min, and the stirring speed is 800-1500 r / min.
[0039] The present application also provides a method for improving the properties of shield tunneling slag, using the above-mentioned shield tunneling foaming agent during the shield tunneling process.
[0040] The embodiments of the present application will be described in detail below in conjunction with specific examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If specific conditions are not specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0041] Example 1
[0042] Example 1 provides a green and environmentally friendly powder non-ionic dispersed foaming agent, including: 600g of sodium dodecylbenzene sulfonate as a foaming agent, 150g of tea saponin as a foaming aid, 220g of coconut oil fatty acid diethanolamide as a stabilizer, 10g of lactic acid as a pH adjuster, and 20g of alkyl glycoside as a lubricant.
[0043] The preparation method of the green and environmentally friendly powder non-ionic dispersed foaming agent of Example 1 comprises:
[0044] (1) In a stirring device, add sodium dodecylbenzene sulfonate, tea saponin, coconut oil fatty acid diethanolamide, lactic acid, and alkyl glycoside. Stir for 15 minutes at a stirring speed of 1000 r / min and mix evenly to obtain a dry powder.
[0045] The green and environmentally friendly powder non-ionic dispersed foaming agent of Example 1 was mixed with water in a mass ratio of 1:16, and then its foaming multiple and foam half-life were tested. The results are shown in Table 1.
[0046] The test method for foam expansion multiple is as follows: weigh 20-30g of foaming agent solution diluted with water into a dried 1000L measuring cylinder, the weight of the foaming agent solution is recorded as m, seal the mouth of the measuring cylinder, hold the measuring cylinder horizontally with both hands, and shake it up and down to make it foam until there is no visible foaming agent solution. After the foaming is completed, let the measuring cylinder stand upright for 1 minute, read the foam volume v, and the foaming multiple is: v / m*ρ, ρ is the density of the foaming agent solution, which is determined according to the density meter method in 4.3 Method 3 of GB / T4472-2011.
[0047] The testing method for foam half-life is as follows: weigh 20-30g diluted foaming agent solution into a dried 1000L measuring cylinder with the foaming agent weight as m, seal the measuring cylinder mouth, hold the measuring cylinder horizontally with both hands, and shake it up and down to make it foam until no foaming agent solution is visible. Start timing after the foaming ends, and the time when the foam volume disappears to half of the initial foam volume is the half-life.
[0048] Example 2
[0049] Example 2 provides a green and environmentally friendly powder non-ionic dispersed foaming agent, including: 600g of sodium dodecylbenzene sulfonate as a foaming agent, 170g of tea saponin as a foaming aid, 200g of coconut oil fatty acid diethanolamide as a stabilizer, 10g of lactic acid as a pH adjuster, and 20g of alkyl glycoside as a lubricant.
[0050] The preparation method of the green and environmentally friendly powder nonionic dispersed foaming agent of Example 2 is the same as that of Example 1. The green and environmentally friendly powder nonionic dispersed foaming agent of Example 2 is mixed with water in a mass ratio of 1:16, and then its foaming multiple and foam half-life are tested. The results are shown in Table 1.
[0051] Example 3
[0052] Example 3 provides a green and environmentally friendly powder non-ionic dispersed foaming agent, including: 600g of sodium dodecylbenzene sulfonate as a foaming agent, 180g of tea saponin as a foaming aid, 190g of coconut oil fatty acid diethanolamide as a stabilizer, 10g of lactic acid as a pH adjuster, and 20g of alkyl glycoside as a lubricant.
[0053] The preparation method of the green and environmentally friendly powder nonionic dispersed foaming agent of Example 3 is the same as that of Example 1. The green and environmentally friendly powder nonionic dispersed foaming agent of Example 3 is mixed with water in a mass ratio of 1:16, and then its foaming multiple and foam half-life are tested. The results are shown in Table 1.
[0054] Example 4
[0055] Example 4 provides a green and environmentally friendly powder non-ionic dispersed foaming agent, including: 600g of sodium dodecylbenzene sulfonate as a foaming agent, 150g of tea saponin as a foaming aid, 210g of coconut oil fatty acid diethanolamide as a stabilizer, 10g of lactic acid as a pH adjuster, and 30g of alkyl glycoside as a lubricant.
[0056] The preparation method of the green and environmentally friendly powder nonionic dispersed foaming agent of Example 4 is the same as that of Example 1. The green and environmentally friendly powder nonionic dispersed foaming agent of Example 4 is mixed with water in a mass ratio of 1:19, and then its foaming multiple and foam half-life are tested. The results are shown in Table 1.
[0057] Example 5
[0058] Example 5 provides a green and environmentally friendly powder non-ionic dispersed foaming agent, including: 600g of sodium dodecylbenzene sulfonate as a foaming agent, 170g of tea saponin as a foaming aid, 190g of coconut oil fatty acid diethanolamide as a stabilizer, 10g of lactic acid as a pH adjuster, and 30g of alkyl glycoside as a lubricant.
[0059] The preparation method of the green and environmentally friendly powder nonionic dispersed foaming agent of Example 5 is the same as that of Example 1. The green and environmentally friendly powder nonionic dispersed foaming agent of Example 5 is mixed with water in a mass ratio of 1:19, and then its foaming multiple and foam half-life are tested. The results are shown in Table 1.
[0060] Example 6
[0061] Example 6 provides a green and environmentally friendly powder non-ionic dispersed foaming agent, including: 590g of sodium dodecylbenzene sulfonate as a foaming agent, 180g of tea saponin as a foaming aid, 190g of coconut oil fatty acid diethanolamide as a stabilizer, 10g of lactic acid as a pH adjuster, and 30g of alkyl glycoside as a lubricant.
[0062] The preparation method of the green and environmentally friendly powder nonionic dispersed foaming agent of Example 6 is the same as that of Example 1. The green and environmentally friendly powder nonionic dispersed foaming agent of Example 6 is mixed with water in a mass ratio of 1:19, and then its foaming multiple and foam half-life are tested. The results are shown in Table 1.
[0063] Example 7
[0064] Example 7 provides a green and environmentally friendly powder non-ionic dispersed foaming agent, including: 580g of sodium dodecylbenzene sulfonate as a foaming agent, 150g of tea saponin as a foaming aid, 240g of coconut oil fatty acid diethanolamide as a stabilizer, 10g of lactic acid as a pH adjuster, and 20g of alkyl glycoside as a lubricant.
[0065] The preparation method of the green and environmentally friendly powder nonionic dispersed foaming agent of Example 7 is the same as that of Example 1. The green and environmentally friendly powder nonionic dispersed foaming agent of Example 7 is mixed with water in a mass ratio of 1:22, and then its foaming multiple and foam half-life are tested. The results are shown in Table 1.
[0066] Example 8
[0067] Example 8 provides a green and environmentally friendly powder non-ionic dispersed foaming agent, including: 5800g of sodium dodecylbenzene sulfonate as a foaming agent, 170g of tea saponin as a foaming aid, 220g of coconut oil fatty acid diethanolamide as a stabilizer, 10g of lactic acid as a pH adjuster, and 20g of alkyl glycoside as a lubricant.
[0068] The preparation method of the green and environmentally friendly powder nonionic dispersed foaming agent of Example 8 is the same as that of Example 1. The green and environmentally friendly powder nonionic dispersed foaming agent of Example 8 is mixed with water in a mass ratio of 1:22, and then its foaming multiple and foam half-life are tested. The results are shown in Table 1.
[0069] Example 9
[0070] Example 9 provides a green and environmentally friendly powder non-ionic dispersed foaming agent, including: 590g of sodium dodecylbenzene sulfonate as a foaming agent, 180g of tea saponin as a foaming aid, 200g of coconut oil fatty acid diethanolamide as a stabilizer, 10g of lactic acid as a pH adjuster, and 20g of alkyl glycoside as a lubricant.
[0071] The preparation method of the green and environmentally friendly powder nonionic dispersed foaming agent of Example 9 is the same as that of Example 1. The green and environmentally friendly powder nonionic dispersed foaming agent of Example 9 is mixed with water in a mass ratio of 1:22, and then its foaming multiple and foam half-life are tested. The results are shown in Table 1.
[0072] Comparative Example 1
[0073] Comparative Example 1 A commercially available finished foaming agent is mixed with water in a recommended mass ratio of 1:19, and then its foaming coefficient and foam half-life are tested. The results are shown in Table 1.
[0074] Comparative Example 2
[0075] Comparative Example 2 provides a green and environmentally friendly powder non-ionic dispersed foaming agent, including: 600g of sodium dodecylbenzene sulfonate as a foaming agent, 150g of tea saponin as a foaming aid, 220g of coconut oil fatty acid diethanolamide as a stabilizer, 10g of lactic acid as a pH adjuster, and 20g of alkyl glycoside as a lubricant.
[0076] The preparation method of the green and environmentally friendly powder non-ionic dispersed foaming agent of Comparative Example 2 comprises:
[0077] (1) In a stirring device, add sodium dodecylbenzene sulfonate, tea saponin, coconut oil fatty acid diethanolamide, lactic acid, and alkyl glycoside. Stir for 15 minutes at a stirring speed of 1000 r / min and mix evenly to obtain a dry powder.
[0078] The green and environmentally friendly powder non-ionic dispersed foaming agent of Comparative Example 2 was mixed with water in a mass ratio of 1:10, and then its foaming multiple and foam half-life were tested. The results are shown in Table 1.
[0079] Comparative Example 3
[0080] Comparative Example 3 provides a green and environmentally friendly powder non-ionic dispersed foaming agent, including: 600g of sodium dodecylbenzene sulfonate as a foaming agent, 150g of tea saponin as a foaming aid, 220g of coconut oil fatty acid diethanolamide as a stabilizer, 10g of lactic acid as a pH adjuster, and 20g of alkyl glycoside as a lubricant.
[0081] The preparation method of the green and environmentally friendly powder non-ionic dispersed foaming agent of Comparative Example 3 comprises:
[0082] (1) In a stirring device, add sodium dodecylbenzene sulfonate, tea saponin, coconut oil fatty acid diethanolamide, lactic acid, and alkyl glycoside. Stir for 15 minutes at a stirring speed of 1000 r / min and mix evenly to obtain a dry powder.
[0083] The green and environmentally friendly powder non-ionic dispersed foaming agent of Comparative Example 3 was mixed with water at a mass ratio of 1:30, and then its foaming multiple and foam half-life were tested. The results are shown in Table 1.
[0084] Comparative Example 4
[0085] Comparative Example 4 provides a powder-type foaming agent, including: 600 g of sodium dodecylbenzene sulfonate as a foaming agent, 150 g of polyethylene glycol as a foaming aid, 220 g of coconut oil fatty acid diethanolamide as a stabilizer, 10 g of lactic acid as a pH adjuster, and 20 g of alkyl glycoside as a lubricant.
[0086] The preparation method of the powder type foaming agent of Comparative Example 4 comprises:
[0087] (1) In a stirring device, add sodium dodecylbenzene sulfonate, coconut oil diethanolamide, polyethylene glycol, lactic acid, and alkyl polyglycoside. Stir for 15 minutes at a stirring speed of 1000 r / min and mix evenly to obtain a dry powder.
[0088] The powdered foaming agent of Comparative Example 4 was mixed with water in a mass ratio of 1:19, and then its foaming multiple and foam half-life were tested. The results are shown in Table 1.
[0089] Comparative Example 5
[0090] Comparative Example 5 provides a powder-type foaming agent, including: 600 g of sodium dodecylbenzene sulfonate as a foaming agent, 150 g of gum arabic as a foaming agent, 220 g of coconut oil fatty acid diethanolamide as a stabilizer, 10 g of lactic acid as a pH adjuster, and 20 g of alkyl polyglycoside as a lubricant.
[0091] The preparation method of the powder type foaming agent of Comparative Example 5 comprises:
[0092] (1) In a stirring device, add sodium dodecylbenzene sulfonate, coconut oil diethanolamide, polyethylene glycol, lactic acid, and alkyl polyglycoside. Stir for 15 minutes at a stirring speed of 1000 r / min and mix evenly to obtain a dry powder.
[0093] The powdered foaming agent of Comparative Example 5 was mixed with water in a mass ratio of 1:19, and then its foaming multiple and foam half-life were tested. The results are shown in Table 1.
[0094] Comparative Example 6
[0095] Comparative Example 6 provides a powder foaming agent, including: 600g of sodium dodecylbenzene sulfonate as a foaming agent, 370g of coconut oil fatty acid diethanolamide as a stabilizer, 10g of lactic acid as a pH adjuster, and 20g of alkyl polyglycoside as a lubricant.
[0096] The preparation method of the powder foam agent of Comparative Example 6 comprises:
[0097] (1) In a stirring device, add sodium dodecylbenzene sulfonate, coconut oil fatty acid diethanolamide, lactic acid, and alkyl polyglycoside. Stir for 15 minutes at a stirring speed of 1000 r / min and mix evenly to obtain a dry powder.
[0098] The powdered foaming agent of Comparative Example 6 was mixed with water in a mass ratio of 1:16, and then its foaming multiple and foam half-life were tested. The results are shown in Table 1.
[0099] Table 1 Formulations and test results of the foaming agents of various embodiments and comparative examples
[0100]
[0101]
[0102] It can be seen from the above Examples 1 to 9 that the foaming multiple and the foam half-life, which are two important indicators of the foaming agent, are significantly improved with the increase of the foaming agent in the present invention. When the amount of the foaming agent is 18% and the dilution ratio is 1:19, the effect is best, the maximum foaming multiple is 29 times, and the half-life is 18 minutes. The foam quality meets the design requirements. In Comparative Example 1, the foaming agent on the market generally has a foaming multiple of 18 times and a half-life of 13 minutes. In Comparative Example 2, when the dilution ratio is 1:10, the foaming multiple and the half-life are lower than those in Example 1. In Comparative Example 3, when the dilution ratio is 1:30, the half-life is significantly shortened. In Comparative Examples 4 and 5 in which the foaming agent is replaced and Comparative Example 6 without the foaming agent, it can be found that the foaming multiple and the half-life are far less than the effects of the embodiments. The present invention is much higher than the data of the existing foaming agent, and because the constituent materials are all green and degradable materials, the environmental pollution is greatly reduced.
[0103] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.
[0104] In addition, those skilled in the art will appreciate that, although some embodiments herein include certain features included in other embodiments but not other features, the combination of features of different embodiments is meant to be within the scope of the present application and form different embodiments. For example, in the above claims, any one of the claimed embodiments may be used in any combination. The information disclosed in this background technology section is intended only to deepen the understanding of the overall background technology of the present application and should not be regarded as an admission or in any form of implication that the information constitutes prior art known to those skilled in the art.
Claims
1. A shield foaming agent, characterized in that: The shield foaming agent comprises dry powder and water, wherein the dry powder comprises, by mass percentage: The mass ratio of the dry powder to the water is 1:15-25.
2. The shield foaming agent according to claim 1, characterized in that: The foaming agent is selected from sodium dodecylbenzene sulfonate and / or sodium lauryl sulfate.
3. The shield foaming agent according to claim 1, characterized in that: The foaming aid is tea saponin.
4. The shield foaming agent according to claim 1, characterized in that: The foam stabilizer is selected from coconut oil fatty acid diethanolamide.
5. The shield foaming agent according to claim 1, characterized in that: The foam lubricant is an alkyl polyglycoside.
6. The shield foaming agent according to claim 1, characterized in that: The pH adjuster is at least one of lactic acid and malic acid.
7. The shield foaming agent according to any one of claims 1 to 6, characterized in that: The shield foaming agent has a foaming multiple of 20-30 and a foam half-life of 15-20 minutes.
8. A method for preparing a shield foaming agent according to any one of claims 1 to 7, characterized in that: include: A foaming agent, a foaming aid, a foam stabilizer, a pH regulator and a foam lubricant are mixed to obtain a dry powder shield foaming agent, and the dry powder shield foaming agent is mixed with water to obtain the shield foaming agent.
9. The method for preparing a shield foaming agent according to claim 8, characterized in that: The mixing time is 10-30 min, and the mixing speed is 800-1500 r / min.
10. A method for improving the properties of shield slag, characterized in that: The shield foaming agent according to any one of claims 1 to 7 is used in a shield tunneling process.