Application of glass fiber composite felt in nucleic acid extraction
By pretreating and two soaking treatments on the glass fiber composite felt, the contamination problem caused by the easy breakage of materials in the existing nucleic acid extraction methods is solved, and the accuracy of nucleic acid extraction is improved. Efficiency, suitable for biomedical research and clinical diagnosis.
Patent Information
- Application Number
- CN202410977996.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-01
AI Technical Summary
In the existing nucleic acid extraction methods, silicone membrane, quartz filter paper and glass fiber filter paper are prone to shatter, resulting in the microflower blockage when the liquid is soaked for too long or the flow rate is too large, limiting the rate and efficiency of nucleic acid extraction and affecting the accuracy of the results. .
Pretreatment and two soaking treatments are used to remove metal, oil, protein and RNase contamination, and used in microfluidic nucleic acid extraction devices to avoid breakage and clogging and ensure the accuracy of the extraction results.
Through the preparation method of glass fiber composite felt, stable use in microfluidic nucleic acid extraction device is achieved, microfluidic blockage is avoided, and the accuracy and efficiency of nucleic acid extraction is improved. It is suitable for biomedical research and clinical diagnosis.
Smart Images

Figure CN118879686A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nucleic acid extraction, in particular to application of glass fiber composite felt in nucleic acid extraction. Background Art
[0002] Nucleic acid extraction methods are usually divided into centrifugal precipitation and solid phase adsorption. The commonly used adsorption medium for solid phase adsorption is silica gel membrane or magnetic beads. Chinese patents CN103173432B and CN111206030B use quartz filter paper and glass fiber filter paper as solid phase adsorption media. The above solid phase adsorption media are all made of silicon dioxide as the main raw material. Because there are a large number of hydroxyl groups on the surface of silicon dioxide, nucleic acids can be selectively adsorbed and released in a suitable buffer, thereby achieving the purpose of separating nucleic acids.
[0003] Automated nucleic acid extraction has been achieved by using magnetic beads to extract nucleic acids. Chinese patents CN114921458A and CN114591824A provide a nucleic acid extraction device based on a microfluidic method, which enables membrane-based solid-phase adsorption media to also achieve automated nucleic acid extraction. Although current silica gel membranes, quartz filter paper, and glass fiber filter paper can be used in such devices, they are easily broken and blocked if they are soaked in liquid for too long or the liquid flow rate is too high, which limits the rate and efficiency of nucleic acid extraction and is not conducive to rapid nucleic acid extraction.
[0004] Fiberglass mat is a thin sheet product made of glass fiber, which is combined together by chemical adhesives or mechanical action. It has good structural stability and strong mechanical properties. It is widely used in the construction industry, automobile industry, shipbuilding industry, and electrical industry, but it is rarely used in the biological field for nucleic acid extraction. Summary of the invention
[0005] The object of the present invention is to provide an application of a glass fiber composite felt in nucleic acid extraction. The present invention performs a first immersion treatment and a second immersion treatment on the glass fiber felt in a first treatment liquid and a second treatment liquid respectively, which can not only eliminate the contamination of the glass fiber felt by metal, grease, protein, and RNA enzyme, but also the prepared glass fiber composite felt will not be broken when used in a microfluidic nucleic acid extraction device, resulting in clogging of the microchannel and affecting the accuracy of the nucleic acid extraction result.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] The invention provides application of glass fiber composite felt in nucleic acid extraction.
[0008] Furthermore, based on the above technical solution, the glass fiber composite felt is applied to a microfluidic nucleic acid extraction device.
[0009] Furthermore, based on the above technical solution, the microfluidic nucleic acid extraction device is a nucleic acid extraction device based on a microfluidic method provided in patent CN114921458A or patent CN114591824A.
[0010] Further, based on the above technical solution, the preparation method of the glass fiber composite felt comprises the following steps:
[0011] S1: pre-treating the glass fiber mat;
[0012] S2: placing the pretreated glass fiber felt in a first treatment liquid for a first immersion treatment;
[0013] S3: placing the glass fiber felt after the first immersion treatment in a second treatment liquid for a second immersion treatment to obtain a glass fiber composite felt.
[0014] Further, based on the above technical solution, in step S1, the preprocessing includes:
[0015] Wash the glass fiber felt with water 1-3 times and dry it;
[0016] And / or, the glass fiber mat has a size of (4-6)×(4-6) cm and a thickness of 10-100 μm;
[0017] And / or, the drying includes: a drying temperature of 20-30° C. and a drying time of 4-6 hours.
[0018] Further, based on the above technical solution, in step S2, the first treatment solution includes the following components by mass percentage:
[0019] 1% to 3% sodium dodecylbenzene sulfonate, 1% to 3% sodium sulfate of fatty alcohol polyoxyethylene ether, 2% to 6% fatty alcohol polyoxyethylene ether, 0.5% to 2% disodium ethylenediaminetetraacetate and 0.5% to 1% dimethyl silicone oil, and the rest is water.
[0020] Further, based on the above technical solution, in step S2, the first soaking treatment includes:
[0021] S21: soaking the pretreated glass fiber mat in the first treatment solution at a soaking temperature of 20-30° C. for 1-2 hours;
[0022] S22: placing the soaked glass fiber felt in the reconfigured first treatment liquid for further soaking according to the operation of step S21;
[0023] S23: taking out the glass fiber felt in the first treatment liquid, and performing washing and drying treatment;
[0024] And / or, in step S23, the drying includes: a drying temperature of 20-30° C. and a drying time of 4-6 hours.
[0025] Further, on the basis of the above technical solution, in step S3, the second treatment liquid includes 0.05-0.1% of diethyl pyrocarbonate by mass percentage, and the rest is water.
[0026] Further, based on the above technical solution, in step S3, the second soaking treatment includes:
[0027] The glass fiber felt after the first soaking treatment is soaked in the second treatment liquid for 1-2 hours at a soaking temperature of 20-30° C., then placed in a high-pressure sterilizer for high-temperature and high-pressure treatment, and dried to obtain a glass fiber composite felt;
[0028] And / or, in the second soaking treatment, the drying includes: a drying temperature of 20-30° C. and a drying time of 4-6 hours.
[0029] Further, based on the above technical solution, the conditions of the high temperature and high pressure treatment include:
[0030] The pressure is 103.4-205.8 kPa, the temperature is 120-132°C, and the time is 15-30 min.
[0031] The application of a glass fiber composite felt provided by the present invention in nucleic acid extraction has the following beneficial effects:
[0032] 1. The present invention performs a first immersion treatment and a second immersion treatment on the glass fiber felt in a first treatment liquid and a second treatment liquid respectively, which can not only eliminate the contamination of the glass fiber felt by metal, grease, protein, and RNA enzyme, but also the prepared glass fiber composite felt will not break and cause microchannel blockage when used in a microfluidic nucleic acid extraction device, thereby affecting the accuracy of the nucleic acid extraction result.
[0033] 2. The present invention uses low-priced and easily available glass fiber felt for nucleic acid extraction result detection in a microfluidic nucleic acid extraction device. The detection result is accurate, and the excellent tensile strength and flexibility of the glass fiber felt can avoid clogging the microchannel in the microfluidic nucleic acid extraction device, providing a more reliable and efficient carrier material for microfluidic nucleic acid extraction technology, which is helpful to promote the development of biomedical research, clinical diagnosis and other fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0035] Figure 1 The untreated glass fiber mat is used for nucleic acid extraction and amplification diagram;
[0036] Figure 2 A diagram of nucleic acid amplification in which the glass fiber composite felt provided in Example 1 of the present invention is used for nucleic acid extraction. DETAILED DESCRIPTION
[0037] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme in the embodiment of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention. The process parameters of the following embodiments that do not specify specific conditions are usually based on conventional conditions.
[0038] The endpoints and any values of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in the present invention.
[0039] According to a first aspect of the present invention, there is provided a use of a glass fiber composite felt in nucleic acid extraction.
[0040] Specifically, glass fiber mat is a thin sheet product made of glass fiber as raw material, which is combined together by chemical adhesives or mechanical action. It has good structural stability and strong mechanical properties and is widely used in the construction industry, automobile industry, shipbuilding industry, and electrical industry. However, there are no reports of its use in nucleic acid extraction in the biological field.
[0041] As an optional embodiment of the present invention, the glass fiber composite felt is applied to a microfluidic nucleic acid extraction device.
[0042] As an optional embodiment of the present invention, the microfluidic nucleic acid extraction device is a nucleic acid extraction device based on a microfluidic method provided in patent CN114921458A or patent CN114591824A.
[0043] Specifically, the silica content in glass fiber accounts for 50% to 65%, with high tensile strength, but insufficient toughness and easy to break. Glass fiber mat made by adding adhesive to glass fiber overcomes this shortcoming. Glass fiber mat contains silica in glass fiber, and has tensile strength and flexibility. Finished products are available on the market, and are low-priced and easy to obtain, making them more suitable for microfluidic nucleic acid extraction devices.
[0044] As an optional embodiment of the present invention, the preparation method of the glass fiber composite felt comprises the following steps:
[0045] S1: pre-treating the glass fiber mat;
[0046] S2: placing the pretreated glass fiber felt in a first treatment liquid for a first immersion treatment;
[0047] S3: placing the glass fiber felt after the first immersion treatment in a second treatment liquid for a second immersion treatment to obtain a glass fiber composite felt.
[0048] Specifically, glass fiber mat cannot be directly used for nucleic acid extraction because it is inevitably contaminated by metal, grease, protein, and RNase during its production process. It needs to be pre-treated to remove impurities and be suitable for nucleic acid extraction.
[0049] In the traditional method, piranha glue is used to pretreat the glass fiber mat. Although piranha glue has a strong ability to remove impurities, it is also extremely corrosive and will destroy the adhesive in the glass fiber mat, thereby destroying the structural stability of the glass fiber mat. It is not suitable for the pretreatment of glass fiber mat.
[0050] Therefore, the present invention provides a method for preparing a glass fiber composite felt, in which the glass fiber felt is subjected to a first immersion treatment and a second immersion treatment in a first treatment liquid and a second treatment liquid, respectively. This can not only eliminate the contamination of the glass fiber felt by metal, grease, protein, and RNA enzyme, but also the prepared glass fiber composite felt will not break when used in a microfluidic nucleic acid extraction device, causing blockage of the microchannel and affecting the accuracy of the nucleic acid extraction result.
[0051] As an optional implementation of the present invention, in step S1, the preprocessing includes:
[0052] Wash the glass fiber felt with water 1-3 times and dry it;
[0053] And / or, the glass fiber mat has a size of (4-6)×(4-6) cm and a thickness of 10-100 μm;
[0054] And / or, the drying includes: a drying temperature of 20-30° C. and a drying time of 4-6 hours.
[0055] Specifically, the present invention needs to strictly limit the drying temperature to 20-30°C because too high a drying temperature may cause changes in the fiber structure of the glass fiber felt, resulting in problems such as fiber fusion, affecting the fiber separability and molding accuracy, thereby causing the strength and elasticity of the glass fiber felt to decrease, further affecting the nucleic acid extraction results when used in a microfluidic nucleic acid extraction device.
[0056] As an optional embodiment of the present invention, the cleaning water includes one or more of deionized water, purified water, and distilled water.
[0057] As an optional embodiment of the present invention, in step S2, the first treatment solution includes the following components by mass percentage:
[0058] 1% to 3% sodium dodecylbenzene sulfonate, 1% to 3% sodium sulfate of fatty alcohol polyoxyethylene ether, 2% to 6% fatty alcohol polyoxyethylene ether, 0.5% to 2% disodium ethylenediaminetetraacetate and 0.5% to 1% dimethyl silicone oil, and the rest is water.
[0059] Specifically, the main function of the first treatment liquid is to remove the oil, protein or metal ion pollution in the glass fiber mat:
[0060] Among them, the role of sodium dodecylbenzene sulfonate is to remove oil and protein pollution in the glass fiber felt. Moreover, after the glass fiber felt is immersed in the treatment solution containing sodium dodecylbenzene sulfonate, the surface activity of sodium dodecylbenzene sulfonate can activate the hydroxyl groups on the surface of the glass fiber felt, making the glass fiber felt more conducive to the adsorption of nucleic acids.
[0061] Furthermore, the sodium fatty alcohol polyoxyethylene ether sulfate and sodium dodecylbenzene sulfonate work synergistically to more effectively remove oil and protein pollution and keep the glass fiber mat clean.
[0062] Furthermore, the fatty alcohol polyoxyethylene ether has excellent cleaning, emulsifying, dispersing and wetting properties. Its main function is to assist in removing oil and protein, while enhancing the permeability and dispersibility of the first treatment liquid, ensuring that the treatment liquid can evenly and fully cover the surface of the glass fiber mat.
[0063] Furthermore, disodium EDTA is a metal chelating agent that can form stable complexes with a variety of metal ions, thereby effectively removing metal ion contamination in glass fiber mats. This is crucial to maintaining the purity of glass fiber mats and the smooth progress of subsequent processing.
[0064] Furthermore, dimethyl silicone oil is a defoaming agent, which can effectively suppress the foam generated by the first treatment liquid during stirring or use, ensuring the smooth progress of the treatment process. Excessive foam will not only affect the treatment effect, but may also have an adverse effect on the equipment.
[0065] As an optional embodiment of the present invention, in step S2, the first soaking treatment includes:
[0066] S21: soaking the pretreated glass fiber mat in the first treatment solution at a soaking temperature of 20-30° C. for 1-2 hours;
[0067] S22: placing the soaked glass fiber felt in the reconfigured first treatment liquid for further soaking according to the operation of step S21;
[0068] S23: taking out the glass fiber felt in the first treatment liquid, and performing washing and drying treatment;
[0069] And / or, in step S23, the drying includes: a drying temperature of 20-30° C. and a drying time of 4-6 hours.
[0070] Specifically, the glass fiber felt obtained in step S21 does not need to be dried, but is directly placed in the reconfigured first treatment liquid for continued immersion. Through continuous immersion, it is ensured that the glass fiber felt fully absorbs and evenly distributes the components in the treatment liquid, further deepening or strengthening the effect of the first immersion.
[0071] As an optional embodiment of the present invention, in step S3, the second treatment solution includes 0.05-0.1% by mass of diethyl pyrocarbonate, and the rest is water.
[0072] Specifically, the diethyl pyrocarbonate in the second treatment solution is an RNase inhibitor, which can react with the histidine residue in the RNase, thereby making it inactive.
[0073] The present invention strictly limits the content of diethyl pyrocarbonate to 0.05-0.1%, because when the content of diethyl pyrocarbonate is less than 0.05%, the activity of RNase cannot be fully inhibited, resulting in RNA being degraded during extraction or storage, affecting the accuracy and reliability of subsequent nucleic acid extraction; if the content of diethyl pyrocarbonate is higher than 0.1%, diethyl pyrocarbonate itself may be difficult to completely remove, and the residue in the RNA sample may interfere with subsequent experiments. Secondly, excessive diethyl pyrocarbonate may react non-specifically with RNA or other components in the experiment, affecting the results of nucleic acid extraction.
[0074] As an optional embodiment of the present invention, in step S3, the second soaking treatment includes:
[0075] The glass fiber felt after the first soaking treatment is soaked in the second treatment liquid for 1-2 hours at a soaking temperature of 20-30° C., then placed in a high-pressure sterilizer for high-temperature and high-pressure treatment, and dried to obtain a glass fiber composite felt;
[0076] And / or, in the second soaking treatment, the drying includes: a drying temperature of 20-30° C. and a drying time of 4-6 hours.
[0077] Specifically, the purpose of the high temperature and high pressure treatment in the present invention is to decompose diethyl pyrocarbonate into carbon dioxide and alcohol, completely remove its toxicity, and ensure the purity and stability of the sample of the glass fiber felt during the nucleic acid extraction process, thereby avoiding inaccurate nucleic acid extraction results due to diethyl pyrocarbonate residues.
[0078] As an optional embodiment of the present invention, the conditions of the high temperature and high pressure treatment include:
[0079] The pressure is 103.4-205.8 kPa, the temperature is 120-132°C, and the time is 15-30 min.
[0080] The present invention will be further described in detail below with reference to specific embodiments and comparative examples.
[0081] Example 1
[0082] Prepare the first treatment solution:
[0083] About 80 mL of pure water was measured and placed in a 250 mL beaker, and placed on a magnetic stirring stand, the speed was set to 500 rpm-800 rpm, and 0.5 g of disodium ethylenediaminetetraacetate, 0.5 mL of dimethyl silicone oil, 1 g of sodium dodecylbenzene sulfonate, 2 mL of fatty alcohol polyoxyethylene ether, and 1 mL of fatty alcohol polyoxyethylene ether sodium sulfate were added in sequence; wherein, each component was added after it was completely dissolved before adding the next component, and finally the volume was made up to 100 mL with pure water to obtain a first treatment liquid.
[0084] Prepare the second treatment solution:
[0085] 99.9 mL of pure water was measured and placed in a 250 mL beaker, 0.1 mL of diethyl pyrocarbonate was added, and the mixture was placed on a magnetic stirring stand, the speed was set to 500 rpm-800 rpm, and the stirring time was 4 h to obtain a second treatment liquid.
[0086] Preparation method of glass fiber composite felt:
[0087] S1: pre-treating the glass fiber mat;
[0088] A glass fiber mat with a size of 5×5 cm and a thickness of 50 μm was washed with pure water for 1-3 times and dried at 25°C for 5 hours;
[0089] S2: placing the pretreated glass fiber felt in a first treatment liquid for a first immersion treatment;
[0090] S21: soaking the pretreated glass fiber felt in the first treatment solution at a soaking temperature of 25° C. for 2 hours;
[0091] S22: placing the soaked glass fiber felt in the reconfigured first treatment liquid for further soaking according to the operation of step S21;
[0092] S23: taking out the glass fiber felt in the first treatment solution, washing it 1-3 times, and drying it at 25° C. for 5 hours;
[0093] S3: placing the glass fiber mat after the first immersion treatment in a second treatment liquid for a second immersion treatment to obtain a glass fiber composite mat;
[0094] The glass fiber felt after the first immersion treatment was immersed in the second treatment liquid for 2 hours at an immersion temperature of 25°C, and then placed in an autoclave for high temperature and high pressure treatment at a pressure of 205.8 kPa and a temperature of 132°C for 20 minutes, and further dried at 25°C for 5 hours to obtain a glass fiber composite felt.
[0095] Example 2
[0096] Prepare the first treatment solution:
[0097] About 80 mL of pure water was measured and placed in a 250 mL beaker, and placed on a magnetic stirring stand. The speed was set to 500 rpm-800 rpm, and 1 g of disodium ethylenediaminetetraacetate, 1 mL of dimethyl silicone oil, 2 g of sodium dodecylbenzenesulfonate, 4 mL of fatty alcohol polyoxyethylene ether, and 2 mL of fatty alcohol polyoxyethylene ether sodium sulfate were added in sequence, wherein each component was completely dissolved before adding the next component, and finally the volume was fixed to 100 mL with pure water to obtain the first treatment liquid.
[0098] Prepare the second treatment solution:
[0099] Measure 99.9 mL of pure water and place it in a 250 mL beaker. Add 0.1 mL of diethyl pyrocarbonate. Place it on a magnetic stirring stand. Set the speed to 500-800 rpm and the time to 4 hours.
[0100] Preparation method of glass fiber composite felt:
[0101] S1: pre-treating the glass fiber mat;
[0102] A glass fiber felt with a size of 4×4 cm and a thickness of 100 μm was washed with pure water for 1-3 times and dried at 20°C for 6 hours;
[0103] S2: placing the pretreated glass fiber felt in a first treatment liquid for a first immersion treatment;
[0104] S21: soaking the pretreated glass fiber felt in the first treatment solution at a soaking temperature of 20° C. for 2 hours;
[0105] S22: placing the soaked glass fiber felt in the reconfigured first treatment liquid for further soaking according to the operation of step S21;
[0106] S23: taking out the glass fiber felt in the first treatment solution, washing it 1-3 times, and drying it at 20° C. for 6 hours;
[0107] S3: placing the glass fiber mat after the first immersion treatment in a second treatment liquid for a second immersion treatment to obtain a glass fiber composite mat;
[0108] The glass fiber felt after the first immersion treatment was immersed in the second treatment liquid for 2 hours at an immersion temperature of 20°C, and then placed in an autoclave for high temperature and high pressure treatment at a pressure of 150 kPa and a temperature of 120°C for 30 minutes, and further dried at 20°C for 6 hours to obtain a glass fiber composite felt.
[0109] Example 3
[0110] Prepare the first treatment solution:
[0111] About 80 mL of pure water was measured and placed in a 250 mL beaker, and placed on a magnetic stirring stand. The speed was set to 500 rpm-800 rpm, and 1 g of disodium ethylenediaminetetraacetate, 1 mL of dimethyl silicone oil, 3 g of sodium dodecylbenzene sulfonate, 6 mL of fatty alcohol polyoxyethylene ether, and 3 mL of fatty alcohol polyoxyethylene ether sodium sulfate were added in sequence, wherein each component was completely dissolved before adding the next component. Finally, the volume was fixed to 100 mL with pure water to obtain the first treatment solution.
[0112] Prepare the second treatment solution:
[0113] Measure 99.9 mL of pure water and place it in a 250 mL beaker. Add 0.1 mL of diethyl pyrocarbonate. Place it on a magnetic stirring stand. Set the speed to 500-800 rpm and the time to 4 hours.
[0114] Preparation method of glass fiber composite felt:
[0115] S1: pre-treating the glass fiber mat;
[0116] A glass fiber felt with a size of 6×6 cm and a thickness of 20 μm was washed with pure water for 1-3 times and dried at 30°C for 4 hours;
[0117] S2: placing the pretreated glass fiber felt in a first treatment liquid for a first immersion treatment;
[0118] S21: soaking the pretreated glass fiber felt in the first treatment solution at a soaking temperature of 30° C. for 1 hour;
[0119] S22: placing the soaked glass fiber felt in the reconfigured first treatment liquid for further soaking according to the operation of step S21;
[0120] S23: taking out the glass fiber felt in the first treatment solution, washing it 1-3 times, and drying it at 30° C. for 4 hours;
[0121] S3: placing the glass fiber mat after the first immersion treatment in a second treatment liquid for a second immersion treatment to obtain a glass fiber composite mat;
[0122] The glass fiber felt after the first immersion treatment was immersed in the second treatment liquid for 1 hour at an immersion temperature of 30°C, and then placed in an autoclave for high temperature and high pressure treatment for 15 minutes at a pressure of 180 kPa and a temperature of 132°C, and further dried at 30°C for 4 hours to obtain a glass fiber composite felt.
[0123] Example 4
[0124] Prepare the first treatment solution:
[0125] About 80 mL of pure water was measured and placed in a 250 mL beaker, and placed on a magnetic stirring stand. The speed was set to 500 rpm-800 rpm, and 0.5 g of disodium ethylenediaminetetraacetate, 2 mL of dimethyl silicone oil, 3 g of sodium dodecylbenzene sulfonate, 4 mL of fatty alcohol polyoxyethylene ether, and 2 mL of fatty alcohol polyoxyethylene ether sodium sulfate were added in sequence, wherein each component was completely dissolved before adding the next component. Finally, the volume was adjusted to 100 mL with pure water to obtain the first treatment solution.
[0126] Prepare the second treatment solution:
[0127] Measure 99.9 mL of pure water and place it in a 250 mL beaker. Add 0.1 mL of diethyl pyrocarbonate. Place it on a magnetic stirring stand. Set the speed to 500-800 rpm and the time to 4 hours.
[0128] Preparation method of glass fiber composite felt:
[0129] S1: pre-treating the glass fiber mat;
[0130] A glass fiber felt with a size of 5×5 cm and a thickness of 10 μm was washed with pure water for 1-3 times and dried at 22°C for 5 hours;
[0131] S2: placing the pretreated glass fiber felt in a first treatment liquid for a first immersion treatment;
[0132] S21: soaking the pretreated glass fiber felt in the first treatment solution at a soaking temperature of 22° C. for 1.5 hours;
[0133] S22: placing the soaked glass fiber felt in the reconfigured first treatment liquid for further soaking according to the operation of step S21;
[0134] S23: taking out the glass fiber felt in the first treatment solution, washing it 1-3 times, and drying it at 22° C. for 5 hours;
[0135] S3: placing the glass fiber mat after the first immersion treatment in a second treatment liquid for a second immersion treatment to obtain a glass fiber composite mat;
[0136] The glass fiber felt after the first immersion treatment was immersed in the second treatment liquid for 1.5 hours at an immersion temperature of 22°C, and then placed in an autoclave for high temperature and high pressure treatment at a pressure of 140 kPa and a temperature of 125°C for 25 minutes, and further dried at 22°C for 5 hours to obtain a glass fiber composite felt.
[0137] Example 5
[0138] Prepare the first treatment solution:
[0139] About 80 mL of pure water was measured and placed in a 250 mL beaker, and placed on a magnetic stirring stand. The speed was set to 500 rpm-800 rpm, and 0.5 g of disodium ethylenediaminetetraacetate, 1 mL of dimethyl silicone oil, 2 g of sodium dodecylbenzene sulfonate, 3 mL of fatty alcohol polyoxyethylene ether, and 2 mL of fatty alcohol polyoxyethylene ether sodium sulfate were added in sequence, wherein each component was completely dissolved before adding the next component. Finally, the volume was adjusted to 100 mL with pure water to obtain the first treatment solution.
[0140] Prepare the second treatment solution:
[0141] Measure 99.9 mL of pure water and place it in a 250 mL beaker. Add 0.1 mL of diethyl pyrocarbonate. Place it on a magnetic stirring stand. Set the speed to 500-800 rpm and the time to 4 hours.
[0142] Preparation method of glass fiber composite felt:
[0143] S1: pre-treating the glass fiber mat;
[0144] A glass fiber felt with a size of 5×5 cm and a thickness of 80 μm was washed with pure water for 1-3 times and dried at 30°C for 4 hours;
[0145] S2: placing the pretreated glass fiber felt in a first treatment liquid for a first immersion treatment;
[0146] S21: soaking the pretreated glass fiber felt in the first treatment solution at a soaking temperature of 30° C. for 2 hours;
[0147] S22: placing the soaked glass fiber felt in the reconfigured first treatment liquid for further soaking according to the operation of step S21;
[0148] S23: taking out the glass fiber felt in the first treatment solution, washing it 1-3 times, and drying it at 30° C. for 4 hours;
[0149] S3: placing the glass fiber mat after the first immersion treatment in a second treatment liquid for a second immersion treatment to obtain a glass fiber composite mat;
[0150] The glass fiber felt after the first immersion treatment was immersed in the second treatment liquid for 2 hours at an immersion temperature of 30°C, and then placed in an autoclave for high temperature and high pressure treatment at a pressure of 200 kPa and a temperature of 130°C for 15 minutes, and further dried at 30°C for 4 hours to obtain a glass fiber composite felt.
[0151] Comparative Example 1
[0152] Compared with Example 1, the main difference between this comparative example is that the glass fiber felt is directly used in nucleic acid extraction without being treated, and the remaining steps and technical parameters are the same as those in Example 1. The results of nucleic acid extraction are shown in Table 1.
[0153] Comparative Example 2
[0154] Compared with Example 1, the main difference between this comparative example is that the glass fiber felt is only treated in the first treatment liquid and not in the second treatment liquid. The remaining steps and technical parameters are the same as those in Example 1. The results of nucleic acid extraction are shown in Table 1.
[0155] Comparative Example 3
[0156] Compared with Example 1, the main difference between this comparative example is that the glass fiber felt is only treated in the second treatment liquid and not in the first treatment liquid. The remaining steps and technical parameters are the same as those in Example 1. The results of nucleic acid extraction are shown in Table 1.
[0157] Comparative Example 4
[0158] Compared with Example 1, the main difference between this comparative example is that during the second immersion treatment, the glass fiber felt is not subjected to high temperature and high pressure treatment, and the remaining steps and technical parameters are the same as those of Example 1. The results of nucleic acid extraction are shown in Table 1.
[0159] Performance comparison experiment
[0160] The glass fiber composite felt prepared in Examples 1-5 and Comparative Examples 1-4 was subjected to a nucleic acid extraction experiment:
[0161] The samples extracted in this example are Hela cells cultured in the laboratory, and the cell concentrations are 10 5 pcs / mL, 10 4 / mL and 10 3 Pieces / mL.
[0162] The lysis solution includes the following components: 1.5 mol / L guanidine thiocyanate, 10 mmol / L trisodium citrate, 0.5% SDS, 10 mmol / L EDTA, 1% triton x-100 and 50% isopropanol; the pH value is maintained at 5.0-5.5;
[0163] The washing solution includes the following components: 0.3 mol / L KCl and 3% PEG8000 solution, with the pH value maintained at 8.0-8.5;
[0164] The eluent includes the following components: 1mmol / LTris, and the pH value is maintained at 8.0-8.5.
[0165] First, according to the nucleic acid extraction method in the prior art, 10 5 pcs / mL, 10 4 / mL and 10 3 The CT values of nucleic acid extraction from three different cell concentrations of cells / mL were 30.15, 33.05, and 36.26, respectively.
[0166] Then, the nucleic acid extraction device based on the microfluidic method provided in the CN114591824A patent was used to perform automated nucleic acid extraction using the glass fiber composite felt prepared in Examples 1-5 and Comparative Examples 1-4. The extracted nucleic acid was used to detect the GAPDH gene. The test results are shown in Table 1.
[0167] Table 1: Results of nucleic acid extraction before and after glass fiber mat treatment
[0168]
[0169] As shown in Table 1, the glass fiber felt in Comparative Example 1 was directly used for nucleic acid extraction without treatment. Figure 1 As shown in the figure, no results were detected. The possible reasons are low nucleic acid extraction efficiency or too many extracted nucleic acid inhibitors (metal ions, proteins, RNA enzymes, oil stains), resulting in no amplification results; while the test results of Example 1 are consistent with the test results of the nucleic acid extraction method in the prior art within the error range, and as shown in the figure, Figure 2 As shown, the amplification effect of the nucleic acid extracted in Example 1 is good, and samples of different concentrations are in a linear relationship.
[0170] As shown in Table 1, compared with Example 1, since the glass fiber felt in Comparative Example 2 was only treated in the first treatment solution and not in the second treatment solution, the RNase in the cell sample did not lose its activity, which interfered with the nucleic acid results. Compared with the detection results of the nucleic acid extraction method in the prior art, there was a large difference, and the nucleic acid extraction results were inaccurate.
[0171] As shown in Table 1, compared with Example 1, since the glass fiber felt in Comparative Example 3 was only treated in the second treatment liquid but not in the first treatment liquid, the oil, protein, metal ions, etc. in the glass fiber felt affected the nucleic acid extraction process and the concentration and purity of the nucleic acid, and the detection results could not be obtained.
[0172] As shown in Table 1, compared with Example 1, in Comparative Example 4, since the glass fiber felt in Comparative Example 4 was not subjected to high temperature and high pressure treatment during the second immersion treatment, the diethyl pyrocarbonate was not decomposed, resulting in undecomposed diethyl pyrocarbonate mixed in the nucleic acid during the nucleic acid extraction process, inhibiting the reverse transcription process of the reagent, reducing the sensitivity of the reagent, and being unfavorable for nucleic acid detection of the sample.
[0173] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. Application of glass fiber composite felt in nucleic acid extraction.
2. The use of the glass fiber composite felt in nucleic acid extraction according to claim 1, characterized in that: The glass fiber composite felt is used in a microfluidic nucleic acid extraction device.
3. The use of the glass fiber composite felt in nucleic acid extraction according to claim 2, characterized in that: The microfluidic nucleic acid extraction device is a nucleic acid extraction device based on a microfluidic method provided in patent CN114921458A or patent CN114591824A.
4. The use of the glass fiber composite felt in nucleic acid extraction according to claim 1, characterized in that: The preparation method of the glass fiber composite felt comprises the following steps: S1: pre-treating the glass fiber mat; S2: placing the pretreated glass fiber felt in a first treatment liquid for a first immersion treatment; S3: placing the glass fiber felt after the first immersion treatment in a second treatment liquid for a second immersion treatment to obtain a glass fiber composite felt.
5. The use of the glass fiber composite felt in nucleic acid extraction according to claim 4, characterized in that: In step S1, the preprocessing includes: Wash the glass fiber felt with water 1-3 times and dry it; And / or, the glass fiber mat has a size of (4-6)×(4-6) cm and a thickness of 10-100 μm; And / or, the drying includes: a drying temperature of 20-30° C. and a drying time of 4-6 hours.
6. The use of the glass fiber composite felt in nucleic acid extraction according to claim 4, characterized in that: In step S2, the first treatment solution includes the following components by mass percentage: 1% to 3% sodium dodecylbenzene sulfonate, 1% to 3% sodium sulfate of fatty alcohol polyoxyethylene ether, 2% to 6% fatty alcohol polyoxyethylene ether, 0.5% to 2% disodium ethylenediaminetetraacetate and 0.5% to 1% dimethyl silicone oil, and the rest is water.
7. The use of the glass fiber composite felt in nucleic acid extraction according to claim 4, characterized in that: In step S2, the first soaking treatment includes: S21: soaking the pretreated glass fiber mat in the first treatment solution at a soaking temperature of 20-30° C. for 1-2 hours; S22: placing the soaked glass fiber felt in the reconfigured first treatment liquid for further soaking according to the operation of step S21; S23: taking out the glass fiber felt in the first treatment liquid, and performing washing and drying treatment; And / or, in step S23, the drying includes: a drying temperature of 20-30° C. and a drying time of 4-6 hours.
8. The use of the glass fiber composite felt in nucleic acid extraction according to claim 4, characterized in that: In step S3, the second treatment solution includes 0.05-0.1% by mass of diethyl pyrocarbonate, and the rest is water.
9. The use of the glass fiber composite felt in nucleic acid extraction according to claim 4, characterized in that: In step S3, the second soaking treatment includes: The glass fiber felt after the first soaking treatment is soaked in the second treatment liquid for 1-2 hours at a soaking temperature of 20-30° C., then placed in a high-pressure sterilizer for high-temperature and high-pressure treatment, and dried to obtain a glass fiber composite felt; And / or, in the second soaking treatment, the drying includes: a drying temperature of 20-30° C. and a drying time of 4-6 hours.
10. The use of the glass fiber composite felt in nucleic acid extraction according to claim 9, characterized in that: The conditions of the high temperature and high pressure treatment include: The pressure is 103.4-205.8 kPa, the temperature is 120-132°C, and the time is 15-30 min.