Thermal compression deformation processing method of low-carbon high-chromium-cobalt martensite stainless bearing steel

By controlling the deformation temperature and strain rate through hot compression deformation processing, the problem of microstructure coarsening of low-carbon, high-chromium, cobalt martensitic stainless bearing steel during high-temperature service was solved, achieving a fine and uniform microstructure, improving material properties, and making it suitable for manufacturing high-strength and high-toughness aerospace bearings for high-temperature service.

CN118879997APending Publication Date: 2024-11-01HUNAN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410960157.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Existing low-carbon, high-chromium-cobalt martensitic stainless bearing steels suffer from reduced strength and toughness due to the coarsening of nanoscale Mo-rich carbides and martensitic substructure, as well as the precipitation of coarse Cr-rich carbides at grain boundaries during long-term high-temperature service, making it difficult to meet the requirements for high-temperature service.

Method used

By controlling the deformation temperature and strain rate, a hot compression deformation process is used to avoid cracking and obtain a fine and uniform microstructure. This process includes steps such as vacuum induction smelting, homogenization treatment, pre-forging, and hot compression deformation. The deformation temperature is controlled at 1000–1100℃, and the strain rate is controlled at 0.1–20 s⁻¹.

Benefits of technology

It effectively avoids micro-cracks during hot working, obtains fine and uniform microstructure, and improves the strength and toughness of the material, making it suitable for manufacturing high-strength and high-toughness aerospace bearings for high-temperature service.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118879997A_ABST
    Figure CN118879997A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of stainless steel hot working, and particularly relates to a hot compression deformation machining method of low-carbon high-chromium-cobalt martensite stainless bearing steel. The hot compression deformation processing method of the low-carbon high-chromium-cobalt martensite stainless bearing steel comprises the following steps: (1) preparing raw materials, and smelting to obtain a low-carbon high-chromium-cobalt martensite stainless bearing steel casting blank; (2) the casting blank is subjected to homogenization and pre-forging treatment, and a hot compression deformation machining blank is obtained; and (3) carrying out hot compression deformation on the material, and carrying out water cooling to obtain a finished product material with a fine grain structure. According to the hot compression deformation processing method of the low-carbon high-chromium-cobalt martensite stainless bearing steel, the deformation resistance can be effectively reduced, cracking in the hot working process is avoided, and a fine and uniform microstructure can be obtained. The method is mainly suitable for manufacturing high-strength and high-toughness aviation bearings serving at the environment temperature of 400 DEG C or above, and has wide application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of stainless steel hot processing, and specifically relates to a hot compression deformation processing method for a low-carbon high-chromium-cobalt martensitic stainless bearing steel, which is mainly suitable for the manufacture of high-strength and high-toughness aviation bearings that serve for a long time in a high-temperature environment above 400°C. Background Art

[0002] As one of the important "bottleneck" technical problems restricting the development of my country's aviation industry, the bottleneck of the preparation and processing technology of aviation bearing steel has been difficult to break through. As a key component used in large quantities on aircraft, aviation bearings need to serve stably under high temperature and high load conditions. This requires that after proper heat treatment, the surface of aviation bearings should have high hardness, strength, rolling contact fatigue performance and corrosion resistance, and the core should have excellent toughness. The mainstream steel grades currently used in my country to manufacture aviation bearings, such as: M50, M50NiL, 9Cr18, etc., are increasingly unable to meet the needs of the service environment.

[0003] In recent years, a new type of low-carbon high-chromium cobalt martensitic stainless bearing steel has attracted more and more attention due to its excellent high-temperature strength, toughness and corrosion resistance after proper heat treatment. After surface carburizing / nitriding treatment, the surface hardness of this steel can be further improved. Its main strengthening and toughening mechanism depends on the nano-scale Mo-rich carbides and fine martensitic substructures precipitated in the martensitic matrix during tempering. However, aviation bearings need to serve stably and safely at high temperatures for a long time. Once they fail, it will not only bring huge economic losses, but also endanger the lives of the people on board. Studies have found that the nano-scale Mo-rich carbides and fine martensitic substructures in low-carbon high-chromium cobalt martensitic stainless bearing steel are prone to coarsening under long-term high-temperature conditions. More seriously, coarse Cr-rich carbides will precipitate at the grain boundaries, significantly reducing the grain boundary strength. The above factors significantly deteriorate the strength and toughness of low-carbon high-chromium cobalt martensitic stainless bearing steel, bringing uncertainty to the service of the bearings.

[0004] Therefore, how to inhibit the coarsening of nano-scale Mo-rich carbides and martensitic substructures and the precipitation of coarse Cr-rich carbides at grain boundaries in low-carbon, high-chromium-cobalt martensitic stainless bearing steel during long-term high-temperature service has become an important issue that needs to be urgently solved in the preparation and processing technology of high-quality aviation bearings. Grain refinement can solve this problem to a large extent, because the refined grain structure can not only provide a significant fine grain strengthening effect, but also inhibit crack propagation, thus improving the strength and toughness of the material at the same time. In addition, the refined grain structure has a higher density of grain boundaries, which are the preferred precipitation sites of carbides, providing more carbide nucleation sites, which can significantly refine the size of precipitated carbides and avoid the deterioration of toughness caused by the precipitation of coarse Cr-rich carbides at grain boundaries. In metal materials, hot working is an effective method to obtain fine and uniform grain structure. Summary of the invention

[0005] In order to overcome the problems existing in the background technology, the purpose of the present invention is to provide a hot compression deformation processing method for low-carbon, high-chromium, cobalt martensitic stainless bearing steel. By controlling process parameters such as deformation temperature and strain rate, the problems of low-carbon, high-chromium, cobalt martensitic stainless bearing steel being difficult to deform and easy to crack during hot processing are solved, and a fine and uniform microstructure can be obtained, thereby improving material properties.

[0006] In order to achieve the above object, the specific technical solution of the present invention is:

[0007] A hot compression deformation processing method for low-carbon high-chromium cobalt martensitic stainless bearing steel can avoid micro cracks in the low-carbon high-chromium cobalt martensitic stainless bearing steel during the hot compression deformation processing by controlling the deformation temperature and the strain rate, and can obtain a fine and uniform microstructure; the hot compression deformation processing method comprises the following steps:

[0008] (1) preparing raw materials according to chemical composition and smelting low-carbon high-chromium-cobalt martensitic stainless bearing steel ingots by vacuum induction + vacuum consumable remelting method;

[0009] (2) homogenizing the low-carbon, high-chromium-cobalt martensitic stainless bearing steel ingot obtained in step (1), and then pre-forging it, and air-cooling it to room temperature to obtain a pre-forged bar;

[0010] (3) mechanically processing the pre-forged bar obtained in step (2) to obtain a hot compression deformation processed blank;

[0011] (4) The blank obtained in step (3) is subjected to hot compression deformation, and water-cooled to room temperature to obtain a finished product of a low-carbon, high-chromium-cobalt martensitic stainless bearing steel material with a fine grain structure.

[0012] The hot compression deformation processing method of the low-carbon high-chromium-cobalt martensitic stainless bearing steel, in step (1), the chemical composition of the low-carbon high-chromium-cobalt martensitic stainless bearing steel is, by mass percentage, C: ≤0.15%, Cr: 13.3-13.5%, Ni: 2.1-2.2%, Co: 13.5-14%, Mo: 3.4-3.5%, V≤0.5%, Si≤0.1%, Nb≤0.05%, Mn≤0.1%, P≤0.01%, S≤0.01%, Fe: balance.

[0013] In the hot compression deformation processing method of the low-carbon high-chromium-cobalt martensitic stainless bearing steel, in step (2), the temperature of the homogenization treatment is controlled at 1200°C for 12 hours; the initial forging temperature of the pre-forging is controlled at 1000-1200°C, the final forging temperature is ≥950°C, and the forging ratio is >5.

[0014] The hot compression deformation processing method of the low-carbon high-chromium-cobalt martensitic stainless bearing steel preferably has an initial forging temperature of 1100-1150°C and a final forging temperature of 1000-1050°C.

[0015] The hot compression deformation processing method of the low-carbon high-chromium-cobalt martensitic stainless bearing steel, in step (4), firstly heat the hot compression deformation processing blank to 1150°C±20°C at a heating rate of 8-12°C / s, and keep it warm for 4-6 minutes; then cool it to the deformation temperature at a cooling rate of 4-6°C / s, the deformation temperature is 1000-1100°C, keep it warm at the deformation temperature for 0.5-2 minutes, and then cool it at a cooling rate of 0.1-20 seconds. -1 The material is hot compressed at a strain rate of , with a deformation of 60-70%.

[0016] The hot compression deformation processing method of the low-carbon high-chromium-cobalt martensitic stainless bearing steel is preferably, firstly, heating the hot compression deformation processing blank to 1150°C at a heating rate of 10°C / s, and keeping it warm for 5 minutes; then cooling it to the deformation temperature at a cooling rate of 5°C / s, the deformation temperature is 1050-1100°C, and after keeping it warm for 1 minute at the deformation temperature, the blank is cooled at a cooling rate of 0.1-1s. -1 The material is hot compressed at a strain rate of , with a deformation of 60%.

[0017] The hot compression deformation processing method of the low-carbon high-chromium-cobalt martensitic stainless bearing steel has a fine grain structure with a grain size range of 5 to 10 μm in the finished low-carbon high-chromium-cobalt martensitic stainless bearing steel material.

[0018] The design concept of the present invention is:

[0019] The present invention processes low-carbon, high-chromium-cobalt martensitic stainless bearing steel through a hot compression deformation processing method, and coordinately controls processing parameters such as deformation temperature and strain rate, which can not only avoid the problems of high-alloy steel being difficult to deform and easy to crack, but also obtain a fine and uniform microstructure, providing a good initial structure for subsequent heat treatment.

[0020] Lower deformation temperature and faster strain rate will improve the work hardening effect of the material, making low-carbon high-chromium cobalt martensitic stainless bearing steel difficult to deform and easy to crack, while higher deformation temperature and slower strain rate are not conducive to the critical dislocation conditions for recrystallization, and are also prone to grain coarsening. The present invention can effectively reduce deformation resistance by accurately controlling hot deformation process parameters such as deformation temperature and strain rate, avoid micro cracks in low-carbon high-chromium cobalt martensitic stainless bearing steel during hot deformation, and can also induce dynamic recrystallization, which is conducive to obtaining fine and uniform microstructure.

[0021] The advantages and beneficial effects of the present invention are:

[0022] The hot compression deformation processing method of the present invention comprises: (1) preparing raw materials, smelting to obtain low-carbon high-chromium-cobalt martensitic stainless bearing steel ingot; (2) homogenizing and pre-forging the ingot to obtain a hot compression deformation processing ingot; (3) hot compression deformation the material, and water cooling to obtain a finished material with a fine grain structure. The hot compression deformation processing method of the low-carbon high-chromium-cobalt martensitic stainless bearing steel can effectively reduce deformation resistance, avoid cracking during hot working, and obtain a fine and uniform microstructure. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 The microstructures of Example 1(a) and Example 2(b) after pre-forging.

[0024] Figure 2 The flow stress curves obtained during the hot compression deformation process of Examples 1 to 8 are shown in FIG.

[0025] Figure 3-Figure 10 The microstructures of Examples 1 to 8 after hot compression deformation processing are shown in order. DETAILED DESCRIPTION

[0026] The present invention is further described in detail below in conjunction with specific embodiments.

[0027] The low-carbon, high-chromium-cobalt martensitic stainless bearing steel of the embodiment is smelted according to the chemical composition formula listed in the present invention, and the specific chemical composition is shown in Table 1.

[0028] Table 1 (the chemical element content in the table is in wt.%)

[0029] C Cr Ni Co Mo V Nb Si Mn P S Fe 0.08 13.4 2.11 13.9 3.45 0.4 0.03 0.05 0.05 0.005 0.005 margin

[0030] The hot compression deformation processing parameters of the low-carbon high-chromium-cobalt martensitic stainless bearing steel in the embodiment are shown in Table 2.

[0031] Table 2

[0032]

[0033]

[0034] The dimensions of the hot compression deformation materials of the embodiments and comparative examples of the present invention are: 8 mm in diameter and 12 mm in height. The materials are subjected to a tissue homogenization treatment using a Gleeble-3800 thermal simulation testing machine, and the hot compression deformation is a single-pass form.

[0035] Example 1

[0036] In this embodiment, the processing parameters are as shown in Table 2.

[0037] (1) 8kg grade low carbon, high chromium and cobalt martensitic stainless bearing steel ingots were prepared by vacuum induction + vacuum consumable remelting method.

[0038] (2) Perform homogenization and pre-forging treatments, and then air-cool to room temperature to obtain a pre-forged bar.

[0039] (3) The pre-forged bar is machined to obtain a hot compression deformation processed blank.

[0040] (4) The material is subjected to hot compression deformation and water-cooled to room temperature to obtain a low-carbon, high-chromium-cobalt martensitic stainless bearing steel with a fine-grained structure.

[0041] Example 2

[0042] In this embodiment, the processing parameters are performed as shown in Table 2. The difference from Embodiment 1 is that the initial forging temperature of this embodiment is 1100° C. and the final forging temperature is 1000° C.

[0043] Example 3

[0044] In this embodiment, the processing parameters are as shown in Table 2. The difference from Embodiment 1 is that the strain rate in this embodiment is 0.1s -1 .

[0045] Example 4

[0046] In this embodiment, the processing parameters are as shown in Table 2. The difference from Example 1 is that the strain rate in this embodiment is 20s -1 .

[0047] Example 5

[0048] In this embodiment, the processing parameters are as shown in Table 2. The difference from Example 1 is that the deformation temperature of this embodiment is 1000°C and the strain rate is 10s -1 .

[0049] Example 6

[0050] In this embodiment, the processing parameters are as shown in Table 2. The difference from Example 1 is that the deformation temperature of this embodiment is 1050°C, the strain rate is 0.1s -1 .

[0051] Example 7

[0052] In this embodiment, the processing parameters are as shown in Table 2. The difference from Example 1 is that the deformation temperature of this embodiment is 1100°C and the strain rate is 0.1s -1 .

[0053] Example 8

[0054] In this embodiment, the processing parameters are as shown in Table 2. The difference from Example 1 is that the deformation temperature of this embodiment is 1100°C and the strain rate is 20s -1 .

[0055] like Figure 1 As shown, the microstructures of Example 1 and Example 2 after pre-forging. Figure 1 It can be seen that when the initial forging temperature is between 1100 and 1150°C and the final forging temperature is between 1000 and 1050°C, the low-carbon, high-chromium-cobalt martensitic stainless bearing steel ingot does not crack after pre-forging, and the forged structure is relatively uniform.

[0056] like Figure 2As shown, the rheological stress of most embodiments increases rapidly in the initial stage of deformation and remains basically unchanged after reaching the peak value. It can be found from Comparative Example 1 and Example 2 that the rheological curves of the two are basically the same, indicating that within the appropriate pre-forging process range, the rheological behavior produced by the subsequent hot compression deformation process is basically consistent with it. It can be found from Comparative Example 1 and Example 3 that although the reduction in strain rate greatly reduces the peak stress, the rheological stress is still high due to the deformation temperature of only 900°C, and the deformation resistance is large. It can be found from Comparative Example 1 and Example 4 that the increase in strain rate can further increase the peak stress, although the increase is small. When the deformation temperature increases to 1000°C, the rheological stress level of Example 5 is basically consistent with that of Example 3, indicating that the increase in deformation temperature can greatly reduce the peak stress and reduce the deformation resistance. For Example 6, its rheological stress is further reduced with the decrease in strain rate and the increase in deformation temperature. The rheological stress of Example 7 is the lowest among all the embodiments, and its rheological stress shows a significant decrease after reaching the peak value, and then maintains at the same level. This indicates that significant dynamic recrystallization occurs in Example 7, making the softening effect stronger than the work hardening effect, resulting in an obvious stress peak in the flow stress curve. In Example 8, because the strain rate is increased compared to Example 7, the flow stress is greatly increased, and the flow stress curve shows more significant jitter, which indicates that the work hardening effect and the dynamic recrystallization softening effect play a leading role in turn.

[0057] like Figure 3-Figure 10 As shown, the microstructure of each embodiment after hot compression deformation processing. Examples 1 to 4 contain obvious banded structures, and small and indistinguishable grains are gathered near the coarse deformed grains. The banded structure in Example 5 still exists, but the coarse deformed grains are clearly visible, and the number of small and indistinguishable grains near them is reduced. Examples 6 and 7 have undergone significant dynamic recrystallization, basically do not contain banded structures, the grains are small and evenly distributed, and the grain size range is 5 to 10μm. Although Example 8 also underwent obvious dynamic recrystallization, many micro cracks were also generated in the matrix due to the excessive deformation rate.

[0058] In summary, by coordinated regulation of processing parameters such as deformation temperature and strain rate within a certain range through this invention, a fine and uniform grain structure can be obtained in a low-carbon, high-chromium-cobalt martensitic stainless bearing steel, and cracking during hot working can be avoided. It has broad application prospects in the manufacture of high-strength and high-toughness aviation bearings that serve at ambient temperatures above 400°C.

[0059] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the present invention. Although the present invention has been described in detail through the above embodiments, it should be understood by those skilled in the art that various changes may be made to the present invention in form and detail without departing from the scope defined in the claims of the present invention.

Claims

1. A hot compression deformation processing method for low-carbon high-chromium-cobalt martensitic stainless bearing steel, characterized in that: By controlling the deformation temperature and strain rate, the generation of micro cracks in the low-carbon high-chromium-cobalt martensitic stainless bearing steel during the hot compression deformation process can be avoided, and a fine and uniform microstructure can be obtained; the hot compression deformation processing method comprises the following steps: (1) preparing raw materials according to chemical composition and smelting low-carbon high-chromium-cobalt martensitic stainless bearing steel ingots by vacuum induction + vacuum consumable remelting method; (2) homogenizing the low-carbon, high-chromium-cobalt martensitic stainless bearing steel ingot obtained in step (1), and then pre-forging it, and air-cooling it to room temperature to obtain a pre-forged bar; (3) mechanically processing the pre-forged bar obtained in step (2) to obtain a hot compression deformation processed blank; (4) The blank obtained in step (3) is subjected to hot compression deformation, and water-cooled to room temperature to obtain a finished product of a low-carbon, high-chromium-cobalt martensitic stainless bearing steel material with a fine grain structure.

2. The hot compression deformation processing method of low-carbon high-chromium-cobalt martensitic stainless bearing steel according to claim 1, characterized in that: In step (1), the chemical composition of the low carbon, high chromium and cobalt martensitic stainless bearing steel is, by mass percentage, C: ≤0.15%, Cr: 13.3-13.5%, Ni: 2.1-2.2%, Co: 13.5-14%, Mo: 3.4-3.5%, V≤0.5%, Si≤0.1%, Nb≤0.05%, Mn≤0.1%, P≤0.01%, S≤0.01%, Fe: balance.

3. The hot compression deformation processing method of low-carbon high-chromium-cobalt martensitic stainless bearing steel according to claim 1, characterized in that: In step (2), the temperature of the homogenization treatment is controlled at 1200° C. for 12 hours; the initial forging temperature of the pre-forging is controlled at 1000-1200° C., the final forging temperature is ≥950° C., and the forging ratio is >5.

4. The hot compression deformation processing method of low-carbon high-chromium-cobalt martensitic stainless bearing steel according to claim 3 is characterized in that: Preferably, the initial forging temperature is 1100-1150°C, and the final forging temperature is 1000-1050°C.

5. The hot compression deformation processing method of low-carbon high-chromium-cobalt martensitic stainless bearing steel according to claim 1, characterized in that: In step (4), the hot compression deformation processing blank is first heated to 1150°C ± 20°C at a heating rate of 8 to 12°C / s and kept at this temperature for 4 to 6 minutes; then cooled to the deformation temperature at a cooling rate of 4 to 6°C / s, the deformation temperature is 1000 to 1100°C, and after being kept at the deformation temperature for 0.5 to 2 minutes, the blank is cooled at a cooling rate of 0.1 to 20 seconds. -1 The material is hot compressed at a strain rate of , with a deformation of 60-70%.

6. The hot compression deformation processing method of low-carbon high-chromium-cobalt martensitic stainless bearing steel according to claim 5, characterized in that: Preferably, the hot compression deformation processing blank is first heated to 1150°C at a heating rate of 10°C / s and kept at this temperature for 5 minutes; then cooled to the deformation temperature at a cooling rate of 5°C / s, and the deformation temperature is 1050-1100°C. After being kept at the deformation temperature for 1 minute, the blank is cooled at a cooling rate of 0.1-1s. -1 The material is hot compressed at a strain rate of , with a deformation of 60%.

7. The hot compression deformation processing method of low-carbon high-chromium-cobalt martensitic stainless bearing steel according to claim 6, characterized in that: In the finished product of low-carbon, high-chromium-cobalt martensitic stainless bearing steel material, the particle size range of fine-grained grains is 5 to 10 μm.