Production method of 730MPa-grade vanadium-containing steel bar

Through the multi-stage cold-controlled process, the grain is refined and the metallographic structure is improved, and the cost increase caused by the large amount of vanadium alloy is solved, and the low-cost production of high-strength steel bars is achieved, with excellent performance and meeting market demand.

CN118880001APending Publication Date: 2024-11-01WUHAN IRON & STEEL GRP ECHENG IRON & STEEL CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410837147.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

While increasing the strength of the steel bar, the use of vanadium alloys in the prior art has increased, resulting in an increase in production costs, and the performance advantages of high-strength steel bars are difficult to meet market demand.

Method used

The new generation of multi-stage cold-controlled process is used to refine grains, improve metallographic structure, induce ferrite phase transformation through four recovery recrystallization and design deformation, control the precipitation of vanadium alloy, reduce the content of vanadium alloy, and improve the yield strength of steel bars and tensile strength.

Benefits of technology

The yield strength of the 730MPa-grade vanadium-containing steel bars produced reaches more than 740MPa and the tensile strength reaches more than 910MPa. They have excellent mechanical properties, which reduces production costs and improves welding performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses a production method of 730MPa-grade vanadium-containing steel bars, and belongs to the technical field of steel bar production. The method comprises the steps of blank preparation and acceptance inspection, billet heating and controlled cooling. Wherein in the controlled cooling process, the rolling starting temperature of a steel billet is controlled to be 950-1050 DEG C, pre-finish rolling, water cooling, finish rolling, water cooling, diameter reducing primary rolling, water cooling, diameter reducing secondary rolling and water cooling are sequentially carried out on the steel billet, the spinning temperature is controlled to be 870-890 DEG C, and the steel billet enters an air cooling roller bed to be cooled. According to the method, the vanadium content in the reinforcing steel bar is controlled, the multi-stage controlled cooling process is controlled, and the temperature return guide groove of 50 m or above is formed among finish rolling, primary diameter reducing rolling and secondary diameter reducing rolling, so that the product performance is improved. The steel bar produced through the method has excellent mechanical properties, the yield strength of the steel bar reaches 740 MPa or above, the tensile strength of the steel bar reaches 910 MPa or above, the percentage elongation after fracture reaches 18%, the maximum elongation reaches 10% or above, and the steel bar has good application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of steel bar production, and specifically relates to a production method of 730MPa grade vanadium-containing steel bars. Background Art

[0002] According to international and domestic steel strength classification standards, the yield strength of high-strength steel is usually defined as 690MPa or 700MPa and above. This means that any steel with a yield strength of 700MPa or more can be classified as high-strength steel. High-strength threaded steel bars are a kind of building material with excellent functions and wide applications. Its application scope includes many fields such as construction engineering, bridge engineering, highway engineering and tunnel engineering, such as high-rise buildings, large frame structures, etc.

[0003] Compared with ordinary steel bars, high-strength threaded steel bars have higher tensile strength and yield strength, can withstand greater loads, and improve the seismic performance and safety of concrete structures. In bridge structures, high-strength threaded steel bars are often used in important parts such as large-span bridges and highway bridges. Their high strength and excellent toughness can effectively improve the bearing capacity and seismic performance of bridges. With the rapid development of my country's infrastructure, the scale of construction continues to increase, and the amount of high-strength steel bars is showing a sharp growth trend. However, to increase the strength of steel bars, it is necessary to consume more vanadium and other alloys, which will increase costs. For example, by adding vanadium alloys to increase the strength of steel bars by about 50MPa, one ton of steel needs to add about 0.2% of vanadium alloys, and the cost increases by about 200 yuan / ton. Therefore, in order to meet market demand requirements, the present invention provides a low-cost and excellent product performance 730MPa grade vanadium-containing steel bar production method. Summary of the invention

[0004] In view of the above deficiencies in the prior art, the purpose of the present invention is to provide a 730MPa grade vanadium-containing steel bar production and rolling method, which refines the grains and improves the metallographic structure by controlling the use of a new generation of multi-stage controlled cooling process, so as to make the austenite transformation more complete and improve product performance.

[0005] To achieve the above purpose, the specific technical solutions of the present invention are as follows:

[0006] A method for producing 730MPa grade vanadium-containing steel bars comprises the following steps:

[0007] 1. Billet preparation and acceptance: According to the chemical composition requirements of steel bars, C: 0.26-0.28%, Si: 0.55-0.70%, Mn: 1.50-1.60%, P≤0025%, S≤0025%, V: 0.10-0.12%, the rest are iron and unavoidable impurity elements, Ceq: 0.55-0.58%, and acceptance is carried out.

[0008] 2. Billet Heating: The heating time of the billet in the heating furnace is 85 - 90 minutes; The heating of the heating furnace is divided into three sections. Among them, the temperature of the preheating section is not higher than 850 °C, the temperature of the heating section is 1130 - 1190 °C, and the temperature of the soaking section is 1180 - 1220 °C; The billet discharging temperature is 950 - 1050 °C.

[0009] 3. Controlled Cooling Process: After the billet heated and discharged from the furnace enters the 50m warming guide channel from the medium rolling at a rolling speed of 16m / s, control the starting rolling temperature to be 950 - 1050 °C and enter the four stands of pre-finishing rolling mills for rolling; After pre-finishing rolling, water cooling through the water is carried out. The water flow rate through the water is 320m 3 / h, and the water pressure through the water is 0.5kg / m 2 ; Control the temperature of the rolled piece to be 900 - 930 °C and enter the finishing rolling mill for rolling; After finishing rolling, water cooling through the water is carried out. The water flow rate through the water is 50m 3 / h, and the water pressure through the water is 0.3kg / m 2 ; After passing through the 65m warming guide channel, control the temperature of the rolled piece to be 890 - 930 °C and enter the first reducing rolling mill at a rolling speed of 24m / s; After the first reducing rolling, water cooling through the water is carried out. The water flow rate through the water is 30m 3 / h, and the water pressure through the water is 0.2kg / m 2 ; After passing through the 50m warming guide channel, control the temperature of the rolled piece to be 880 - 920 °C and enter the second reducing rolling mill at a rolling speed of 37.5m / s; After the second reducing rolling, water cooling through the water is carried out. The water flow rate through the water is 30m 3 / h, and the water pressure through the water is 0.2kg / m 2 ; Control the laying temperature to be 870 - 910 °C and lay the wire into the air-cooling roller table for cooling.

[0010] Preferably, the acceptance process further includes carefully checking the furnace number, grade, number of pieces and weight according to the billet transfer card, and only after confirming that there is no error can the overhead crane be commanded to load the material. At the same time, each billet entering the furnace should be visually inspected one by one, and only when the cross-section, shape, size, surface quality, etc. meet the specified requirements can the steel be loaded into the furnace.

[0011] Preferably, the layout of the water tanks for water cooling through the water is as follows: Two groups of water tanks are set for water cooling through the water after pre-finishing rolling and after finishing rolling; One group of water tanks is set for water cooling through the water after the first reducing rolling; Two groups of water tanks are set for water cooling through the water after the second reducing rolling.

[0012] Preferably, two groups of fans are used for air-cooling roller table cooling, and each group of fans is arranged in a "pin" shape by centrifugal fans, and the opening degree of the fans is 40 - 70%.

[0013] Preferably, the speed of the first section of the roller table in the air-cooling roller table cooling is 0.70m / s, and the speeds of the following 12 sections of the roller table are all 0.75m / s.

[0014] The role of the vanadium alloy in the method of the present invention is to refine the grain structure of the steel, improve the strength, toughness and wear resistance of the steel. When vanadium melts into austenite at high temperature, it can increase the hardenability of the steel.

[0015] In the controlled cooling process of the method of the present invention, the function of the temperature recovery guide groove between the finishing rolling, the first diameter reduction and the second diameter reduction is to allow the grain-refined rolled piece to recover through a sufficient distance and time to allow the grains to grow again, so that the next deformation can produce better grain crushing and refinement effects, and greatly improve the yield strength of the finished product; a high-power fan is arranged behind the wire laying machine to control the cooling speed of the rolled piece after rolling, so that it can be quickly cooled to the phase change area, prevent the austenite grains from growing rapidly, and ensure that the surface does not enter the martensite and bainite transformation areas; the placement of the herringbone fan can make the fan air volume at the high-temperature overlap on both sides of the coil larger, the cooling effect is better, and the stability of the performance of the same circle of steel bars is guaranteed.

[0016] The present invention refines grains and improves metallographic structure by controlling a new generation of multi-stage controlled cooling process, so as to make austenite transformation more complete and improve product performance; the rolled piece undergoes four recovery recrystallizations during deformation to limit grain growth; and by designing the deformation amount of the last two passes, the deformation induces ferrite phase transformation, so that the crushing and deformation of the grains achieve the effect of grain refinement; three sections of temperature recovery guide grooves with a length of 50m or more are used to ensure that the rolled piece is returned to the two-phase region after rolling for the next rolling, and the toughness and strength of the coil are controlled by rapid cooling after rolling to improve the performance of the steel bar; a controlled cooling device is arranged after the finished rolling mill to control the cooling speed of the rolled piece after rolling, so that it is quickly cooled to the phase transformation region to prevent the rapid growth of austenite grains, while ensuring that the surface does not enter the martensite and bainite transformation region, and that the base circle does not have tempered martensite and a closed-loop structure different from the matrix.

[0017] Compared with the prior art, the present invention is beneficial in that:

[0018] (1) The present invention improves the performance of steel bars by controlling a multi-stage controlled cooling process. The yield strength of the 730MPa grade vanadium-containing steel bars produced reaches above 740MPa, the tensile strength reaches above 910MPa, the elongation after fracture reaches 18%, the maximum elongation reaches above 10%, and the mechanical properties are excellent.

[0019] (2) Compared with ordinary HTRB630 steel bars, the vanadium-containing steel bars of the present invention have lower vanadium alloy content and better mechanical properties, thereby reducing production costs and improving the welding performance of the steel bars.

[0020] (3) The present invention adopts a multi-stage controlled cold rolling line layout, a long-distance temperature return guide groove to ensure two-phase rolling, and strict control of the rolling controlled cold process parameters to promote the precipitation strengthening effect of vanadium alloy. On the basis of the chemical composition of HTRB630 steel bars, high-strength threaded steel bars with better mechanical properties, smaller performance differences in the same circle, and lower alloy composition are obtained. DETAILED DESCRIPTION

[0021] The following is a clear and complete description of the technical solution of the present invention in combination with the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work belong to the scope of protection of the present invention. Any equivalent transformation or substitution made by those skilled in the art based on the following implementation methods belongs to the protection scope of the present invention.

[0022] The present invention provides a method for producing a 730MPa grade vanadium-containing steel bar, comprising the following steps:

[0023] 1. Billet preparation and acceptance: According to the chemical composition requirements of steel bars, C: 0.26-0.28%, Si: 0.55-0.70%, Mn: 1.50-1.60%, P≤0025%, S≤0025%, V: 0.10-0.12%, the rest are iron and unavoidable impurity elements, Ceq: 0.55-0.58%, and acceptance is carried out.

[0024] 2. Billet heating: The heating time of the billet in the heating furnace is 85-90 minutes; the heating in the heating furnace is divided into three sections, among which the preheating section temperature is not higher than 850℃, the heating section temperature is 1130-1190℃, and the soaking section temperature is 1180-1220℃; the billet out-of-furnace temperature is 950-1050℃.

[0025] 3. Controlled cooling process: The heated billet is rolled into a 50m temperature return guide trough at a rolling speed of 16m / s, and the rolling temperature is controlled to be 950-1050℃ before entering the pre-finishing rolling four-stand rolling mill; after pre-finishing rolling, water cooling is performed with a water flow rate of 320m 3 / h, water penetration pressure 0.5kg / m 2 ; Control the temperature of the rolled piece to 900-930℃ before entering the finishing mill for rolling; After finishing rolling, cool it with water, and the water flow rate is 50m 3 / h, water penetration pressure 0.3kg / m 2 ; After passing through the 65m temperature return guide groove, the rolled piece temperature is controlled at 890-930℃ and enters the reducing mill at a rolling speed of 24m / s; after the reducing mill, water cooling is performed, and the water flow rate is 30m 3 / h, water penetration pressure 0.2kg / m 2 ; After passing through the 50m temperature return guide groove, the rolled piece temperature is controlled at 880-920℃ and enters the second diameter reducing mill at a rolling speed of 37.5m / s; after the second diameter reducing mill, water cooling is performed, and the water flow rate is 30m 3 / h, water penetration pressure 0.2kg / m 2 ; Control the spinning temperature to 870-910℃ and then the spinning enters the air-cooled roller for cooling.

[0026] The acceptance process also includes carefully checking the furnace number, grade, number of pieces, and weight according to the billet transfer card. Only after confirmation can the operator command the overhead crane to load the materials. At the same time, each billet to be charged into the furnace should be visually inspected one by one. The billet can be charged into the furnace only when its cross-section, shape, size, surface quality, etc. meet the specified requirements.

[0027] The layout of the water tanks for the water-through cooling is as follows: two sets of water tanks are provided for both the post-pre-finishing rolling and post-finishing rolling water-through cooling; one set of water tanks is provided for the water-through cooling after the first reducing rolling; two sets of water tanks are provided for the water-through cooling after the second reducing rolling.

[0028] For the air-cooled roller table cooling, two sets of fans are used. Each set of fans consists of three centrifugal fans arranged in a "pin" shape, and the fan opening degree is 40 - 70%. In the following embodiments, the fan opening degrees of each set of fans are set to 40%, 70%, and 70% respectively.

[0029] In the air-cooled roller table cooling, the speed of the first section of the roller table is 0.70 m / s, and the speeds of the subsequent 12 sections of the roller table are all 0.75 m / s.

[0030] Examples 1 - 5

[0031] In this example, 730 MPa grade vanadium-containing steel bars are produced by the above method. The details are shown in Tables 1 - 4.

[0032] Comparative Examples 1 - 2

[0033] In this comparative example, vanadium-containing steel bars are produced by the above method. The difference is that in this comparative example, no water tank is used for water cooling between the first reducing rolling and the second reducing rolling. The details are shown in Tables 1 - 4.

[0034] Comparative Examples 3 - 4

[0035] In this comparative example, vanadium-containing steel bars are produced by the above method. The difference is that in this comparative example, the vanadium content exceeds the scope of the present invention. The details are shown in Tables 1 - 4.

[0036] Comparative Example 5

[0037] In this comparative example, vanadium-containing steel bars are produced by the above method. The difference is that in this comparative example, the heating and soaking temperatures of ordinary spiral ribbed bars are adopted. The details are shown in Tables 1 - 4.

[0038] Comparative Example 6

[0039] In this comparative example, vanadium-containing steel bars are produced by the above method. The difference is that in this comparative example, a 20-meter-long warming guide groove is used between before pre-finishing rolling, between finishing rolling and the first reducing rolling, and between the first reducing rolling and the second reducing rolling. The details are shown in Tables 1 - 4.

[0040] Table 1: Chemical Compositions (%) of Vanadium-Containing Steel Bars in Examples 1 - 5 and Comparative Examples 1 - 6

[0041]

[0042] Table 2: Heating temperature control of steel billets containing vanadium steel bars in Examples 1-5 and Comparative Examples 1-6 (°C)

[0043]

[0044] Table 3: Temperature control of cooling process of vanadium-containing steel bars in Examples 1-5 and Comparative Examples 1-6 (°C)

[0045]

[0046] Table 4: Performance parameters of vanadium-containing steel bars of Examples 1-5 and Comparative Examples 1-6

[0047]

[0048] By comparing Examples 1-5 with Comparative Examples 1-2, it can be seen that the yield strength and tensile strength of the steel bars can be significantly improved by setting the vanadium content of the steel bars within the range of 0.10-0.12% and using a multi-stage controlled cooling process during rolling; the steel bar composition of Comparative Examples 3-4 is basically the same as the ordinary HTRB630 coil produced in industry, and by comparing Examples 1-5 with Comparative Examples 3-4, it can be seen that the vanadium alloy composition of the high-strength steel bars produced by the method of the present invention is lower; compared with ordinary HTRB630 coils, the cost can be reduced by about 8 yuan / ton, and the steel bars have higher yield strength and tensile strength; by comparing Examples 1-5 with Comparative Example 5, it can be seen that in the billet heating stage, the heating section temperature and the soaking section temperature are low, which will cause the yield strength of the steel bars produced to fail to meet the requirement of >730MPa; by comparing Examples 1-5 with Comparative Example 6, it can be seen that in the water-through cooling of the multi-stage controlled cooling, the three sections of temperature return guide grooves with a length of 50m or more are set, which can effectively increase the strength of the steel bars to more than 740MPa;

[0049] In summary, based on the composition of ordinary HTRB630 coiled steel bar, the present invention further controls the vanadium alloy content, and improves the performance of the steel bar while reducing the production cost by controlling the multi-stage controlled cooling process. The 730MPa grade vanadium-containing steel bar produced has a yield strength of more than 740MPa, a tensile strength of more than 910MPa, an elongation after fracture of 18%, a maximum elongation of more than 10%, and excellent mechanical properties.

[0050] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for producing 730MPa grade vanadium-containing steel bars, characterized in that: It includes the following steps: S1. Blank preparation and inspection: In accordance with the requirements of the chemical composition of the steel bar, C: 0.26 - 0.28%, Si: 0.55 - 0.70%, Mn: 1.50 - 1.60%, P ≤ 0.025%, S ≤ 0.025%, V: 0.10 - 0.12%, and the rest are iron and inevitable impurity elements, Ceq: 0.55 - 0.58%, carry out the inspection; S2. Steel billet heating; S3. Controlled cooling process: After the steel billet heated and discharged from the furnace enters the 50m warming guide groove from the medium rolling at a rolling speed of 16m / s, control the starting rolling temperature to be 950 - 1050°C and enter the four stands of the pre-finishing mill for rolling, with water spray cooling; control the temperature of the rolled piece to be 900 - 930°C and enter the finishing mill for rolling, with water spray cooling; after passing through the 65m warming guide groove, control the temperature of the rolled piece to be 890 - 910°C and enter the first reducing mill, with water spray cooling; after passing through the 50m warming guide groove, control the temperature of the rolled piece to be 880 - 920°C and enter the second reducing mill, with water spray cooling; control the laying temperature to be 870 - 910°C and lay the wire into the air-cooling roller table for cooling.

2. The method for producing a 730MPa grade vanadium-containing steel bar according to claim 1, characterized in that: The heating time of the steel billet is 85 - 90 minutes. The temperature of the preheating section of the steel billet heating is not higher than 850°C, the heating section temperature is 1130 - 1190°C, the soaking section temperature is 1180 - 1220°C, and the steel billet discharging temperature is 950 - 1050°C.

3. The method for producing a 730MPa grade vanadium-containing steel bar according to claim 1, characterized in that: The water flow rate of the water cooling after pre-finishing rolling is 320m 3 / h, water penetration pressure is 0.5kg / m 2 .

4. The method for producing a 730MPa grade vanadium-containing steel bar according to claim 1, characterized in that: The water flow rate of the water cooling after the finishing rolling is 50m 3 / h, water penetration pressure is 0.3kg / m 2 .

5. The method for producing a 730MPa grade vanadium-containing steel bar according to claim 1, characterized in that: The water flow rate of the water cooling after the first and second diameter reducing rolling is 30m 3 / h, the water penetration pressure is 0.2kg / m 2 .

6. The method for producing a 730MPa grade vanadium-containing steel bar according to claim 1, characterized in that: The air-cooling roller table cooling uses two groups of fans. Each group of fans consists of three centrifugal fans arranged in a "pin" shape, and the fan opening degree is 40 - 70%.

7. The method for producing a 730MPa grade vanadium-containing steel bar according to claim 1, characterized in that: In the air-cooling roller table cooling, the speed of the first section of the roller table is 0.70m / s, and the speeds of the subsequent 12 sections of the roller table are all 0.75m / s.

Citation Information

Cited By

  • Production method for improving surface corrosion of HRB400E deformed steel bar

    CN119972833A