Preparation method of gallium-based liquid metal
Gallium-zinc alloys were prepared from gallium-containing waste by a method of acid leaching-iron ion reduction-pH adjustment-solid-liquid separation-acid dissolution-introduction of chloride ions-single-stage ion exchange-desorption-alkali dissolution-electrolysis. This method solves the problems of long and complex processes in the preparation of gallium-based liquid metals and realizes an efficient and simple gallium extraction and purification process.
Patent Information
- Application Number
- CN202410981244.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-01
AI Technical Summary
Existing technologies for preparing gallium-based liquid metals involve long and complex processes, and the gallium extraction efficiency is low, making it difficult to achieve effective utilization.
Gallium-zinc alloys are synthesized directly from gallium-containing waste using a method of acid leaching, iron ion reduction, pH adjustment, solid-liquid separation, acid dissolution, introduction of chloride ions, single-stage ion exchange, desorption, alkali dissolution, and electrolysis. The purity and recovery rate of gallium are improved through multiple desorption and washing processes.
The efficient preparation of gallium-based liquid metal was achieved, with gallium content ≥95wt% and zinc content 1-5wt%. The overall gallium and zinc yields were 85-95%, and the process was short with good impurity removal effect.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of gallium alloys, and in particular to a method for preparing gallium-based liquid metal. Background Art
[0002] Gallium is a rare metal with similar properties to aluminum, indium and thallium. It has a metallic luster, is soft and ductile. Rare metal gallium is an important strategic resource. A series of compound semiconductor materials, electronic optical materials, new functional materials, special alloys and organic metal compounds prepared with gallium metal as the matrix are important basic supporting materials in the fields of modern electronic computers, communications, aerospace, new energy, medicine and health, and military industry. About 90% of the gallium in the world is recovered from the production process of alumina, with a mature industrial chain. At the same time, gallium is also enriched in the process of zinc smelting and coal ash, but the gallium enriched in these two raw materials has not been industrialized due to the long extraction process and high cost. In terms of traditional technology, the first step is to smelt gallium metal and then prepare gallium-based alloys.
[0003] There are many kinds of valuable metals in Panxi area. Gallium is associated with V, Fe, Ti and other elements in Panxi mines. At present, the extraction of gallium is mainly carried out with vanadium tailings as raw materials. In the process of gallium extraction from vanadium tailings, due to its complex composition, low direct acid leaching rate, high acid consumption, a large number of by-products that are difficult to utilize, and a long process route, this route has not actually been put into industrial production. Therefore, in order to achieve the effective extraction and utilization of gallium, it is of great significance to provide a method for directly preparing gallium-based alloys. Summary of the invention
[0004] The technical problem solved by the present invention is to provide a method for preparing gallium-based liquid metal. The preparation method provided by the present application can utilize gallium-containing waste to directly synthesize gallium-zinc alloy, and has a high gallium content, a short gallium extraction process, and a good impurity removal effect.
[0005] In view of this, the present application provides a method for preparing gallium-based liquid metal, comprising the following steps:
[0006] S1) acid leaching gallium-containing waste to obtain an acidic leaching solution; the gallium-containing waste comprises 89-95wt% Fe oxide, 0-2wt% Si, 1-5wt% ZnO, and 200-600g / t Ga;
[0007] S2) mixing the acidic leachate and iron powder, performing solid-liquid separation after the reaction, and obtaining a gallium-containing leachate; adjusting the pH to 2-5 using a saturated NaOH solution, and performing solid-liquid separation again; and acid-dissolving the solid obtained by the solid-liquid separation again to obtain an acid solution;
[0008] S3) adding a water-soluble chloride salt to the acid solution, performing a single-stage ion exchange after the reaction to obtain a gallium-loaded ion exchange resin, and washing the ion exchange resin;
[0009] S4) performing a first desorption on the ion exchange resin washed in step S3), and performing a first washing on the ion exchange resin obtained by the first desorption;
[0010] S5) adjusting the pH of the liquid obtained in step S4) and performing solid-liquid separation, dissolving the obtained solid in alkali, and performing solid-liquid separation again;
[0011] S6) electrolyzing the liquid phase obtained in step S5) to obtain a gallium-based liquid metal; the gallium-based liquid metal contains ≥95wt% gallium and 1-5wt% zinc.
[0012] Preferably, step S4) also includes a second desorption and a third desorption, specifically:
[0013] performing a first desorption on the ion exchange resin after washing in step S3), and performing a first washing on the ion exchange resin obtained by the first desorption;
[0014] Desorbing the ion exchange resin after the first washing for a second time, and washing the obtained ion exchange resin for a second time;
[0015] The ion exchange resin after the second washing is subjected to a third desorption.
[0016] Preferably, step S6) further includes:
[0017] One or more of gallium, zinc, indium and tin are added to the obtained gallium-based liquid metal.
[0018] Preferably, in step S1), the leaching agent for acid leaching includes one or more of sulfuric acid, oxalic acid, nitric acid and phosphoric acid, the concentration of the leaching agent is 50-500 g / L, the time of the acid leaching is 0.5-6 h, the temperature is 5-100° C., and the liquid-to-solid ratio of the acid leaching is (10-0.1):1.
[0019] Preferably, in step S2), the ratio of the molar amount of iron in the leaching solution to the molar amount of iron powder is (0.5-1.5):1; and the solid-liquid separation method is suction filtration, filter pressing or centrifugation.
[0020] Preferably, in step S3), the water-soluble chloride salt includes one or more of sodium chloride, potassium chloride and ammonium chloride, and the chloride ion concentration of the water-soluble chloride salt in the gallium-containing leachate is 0.5-20 g / L.
[0021] Preferably, in step S3), the ion exchange resin of the single-stage ion exchange includes one or more of polyurethane, tributyl phosphate leaching resin, tributyl phosphate-n-heptane and LSC-900, and the volume ratio of the ion exchange resin to the gallium-rich solution after the reaction is 0.01-1.
[0022] Preferably, the pH of the desorption medium for the first desorption is 5 to 9, and the desorption medium includes one of a dilute sulfuric acid solution, an acetic acid solution, a dilute hydrochloric acid solution and a sodium hydroxide solution.
[0023] Preferably, in step S5), the pH is adjusted to 3.5-6, and the alkali-soluble reagent includes potassium hydroxide or sodium hydroxide.
[0024] Preferably, the anode material of the electrolysis includes graphite, platinum, stainless steel, lead, silver, titanium alloy, tungsten or molybdenum, the cathode material includes copper indium alloy, indium gallium alloy or stainless steel, the electrolysis temperature is 10-100°C, and the current density is 30-1000A / cm 2 .
[0025] The present application provides a method for preparing gallium-based liquid metal, which firstly acid-leaches gallium-containing waste to dissociate gallium from gallium-containing waste to obtain gallium-containing acidic leachate, then mixes it with iron powder to reduce trivalent iron ions in the leachate to divalent iron ions, and then separates the solid and liquid to obtain gallium-containing leachate, adjusts the pH with saturated sodium hydroxide solution, obtains gallium-rich solid after solid-liquid separation, acid-dissolves the gallium-rich solid, and then introduces chloride ions to perform single-stage ion exchange to achieve gallium-iron separation, obtains gallium-loaded ion exchange resin, and then washes it to further remove impurities and reduce the content of impurities therein, and then desorbs the gallium ion exchange resin with low impurity content for the first time, and then performs the first washing to make the gallium purity higher, and then performs alkaline dissolution to completely remove iron in the organic phase to obtain gallium-rich hydroxide, and finally performs electrolysis to obtain high-purity gallium-based liquid metal. In the above-mentioned gallium-based liquid metal preparation process, gallium-zinc alloy is directly synthesized using gallium-containing waste, the gallium extraction process is short, the impurity removal effect is good, and the gallium content in the obtained gallium-based liquid metal is high. DETAILED DESCRIPTION
[0026] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.
[0027] In view of the problems of long process and complicated technology in the preparation of gallium-based liquid metal in the prior art, the present application uses gallium-containing waste as raw material, and realizes the preparation of gallium-zinc alloy by acid leaching-iron ion reduction-pH adjustment, solid-liquid separation-acid dissolution-introduction of chloride ions-single-stage ion exchange-desorption-alkali dissolution-electrolysis and other processes. It has the advantages of short process, simple technology and high gallium content. Specifically, the embodiment of the present invention discloses a method for preparing gallium-based liquid metal, comprising the following steps:
[0028] S1) acid leaching gallium-containing waste to obtain an acidic leaching solution; the gallium-containing waste comprises 89-95wt% Fe oxide, 0-2wt% Si, 1-5wt% ZnO, and 200-600g / t Ga;
[0029] S2) mixing the acidic leachate and iron powder, performing solid-liquid separation after the reaction, and obtaining a gallium-containing leachate; adjusting the pH to 2-5 using a saturated NaOH solution, and performing solid-liquid separation again; and acid-dissolving the solid obtained by the solid-liquid separation again to obtain an acid solution;
[0030] S3) adding a water-soluble chloride salt to the acid solution, performing a single-stage ion exchange after the reaction to obtain a gallium-loaded ion exchange resin, and washing the ion exchange resin;
[0031] S4) performing a first desorption on the ion exchange resin washed in step S3), and performing a first washing on the ion exchange resin obtained by the first desorption;
[0032] S5) adjusting the pH of the liquid obtained in step S4) and performing solid-liquid separation, dissolving the obtained solid in alkali, and performing solid-liquid separation again;
[0033] S6) electrolyzing the liquid phase obtained in step S5) to obtain a gallium-based liquid metal; the gallium-based liquid metal contains ≥95wt% gallium and 1-5wt% zinc.
[0034] In the process of preparing gallium-based liquid metal, the present application firstly acid-leaches gallium-containing waste to obtain an acidic leaching solution; the acid leaching is used to dissociate gallium from gallium-containing waste to obtain gallium-containing leaching solution. The gallium-containing waste in the present application is selected from solid waste in the vanadium-titanium magnetite beneficiation process, more specifically selected from vanadium-extracting converter dust, which includes: 89-95wt% Fe oxide, 0-2wt% Si, 1-5wt% ZnO, 200-600g / t Ga. The leaching agent of the acid leaching can be one or more of sulfuric acid, oxalic acid, nitric acid and phosphoric acid, that is, the leaching agent can be selected from sulfuric acid, oxalic acid, nitric acid or phosphoric acid, or it can be a mixture of two or more of sulfuric acid, oxalic acid, nitric acid and phosphoric acid; its concentration is 50-500g / L, specifically, the concentration of the leaching agent is 60-450g / L, more specifically, the concentration of the leaching agent is 100-400g / L. The acid leaching time is 0.5 to 6 hours, specifically, the acid leaching time is 1 to 4.5 hours. The acid leaching temperature is 5 to 90°C, specifically, the acid leaching temperature is 10 to 75°C. The liquid-to-solid ratio of the acid leaching is (10 to 0.1):1, specifically, the liquid-to-solid ratio of the acid leaching is (9 to 1):1, more specifically, the liquid-to-solid ratio of the acid leaching is (7 to 3):1. Stirring can be introduced during the acid leaching process, and there is no particular restriction on the form of stirring. The stirring rate is 0 to 500 rpm, specifically, the stirring rate is 50 to 400 rpm.
[0035] The present application then mixes the above-mentioned acidic leachate and iron powder to reduce the trivalent iron ions in the acidic leachate to divalent iron ions to obtain a gallium-containing leachate and a divalent iron solution. In this process, the ratio of the molar amount of iron in the acidic leachate to the molar amount of iron powder is (0.5-1.5):1, specifically, the ratio of the molar amount of iron to the molar amount of iron powder is (0.6-1.1):1, more specifically, the ratio of the molar amount of iron to the molar amount of iron powder is (0.8-1.0):1, and the reduced iron powder is slowly added until the leachate is tested for no color change by thiocyanate. During the addition of the reduced iron powder, stirring and heating can be performed to accelerate the reaction rate of the reduced iron powder with the trivalent iron in the leachate. After the leachate is tested for no color change by thiocyanate, solid-liquid separation is performed, and the residue can be separated from the leachate by suction filtration, filter pressing, centrifugation, etc., but is not limited to the above separation method.
[0036] The present application further uses a saturated NaOH solution to adjust the pH of the gallium-containing leaching solution to 2-5, and performs solid-liquid separation again. At this time, the liquid of the solid-liquid separation is a ferrous chloride solution, and the gallium content in the solid is about 0.1-0.5wt%, and the zinc content is 5-10wt%; the solid obtained above is acid-dissolved again to obtain an acid solution, and the gallium content in the obtained acid solution is 200-500ppm, and the zinc content is 2-5g / L.
[0037] According to the present invention, a water-soluble chloride salt is then added to the above acid solution, and a gallium-containing leachate containing chloride ions is obtained after the reaction. The introduction of chloride ions is to combine with trivalent gallium to form gallium tetrachloride with a negative charge, so as to better combine with the ion exchange resin or form ion exchange. The water-soluble chloride salt includes one or more of sodium chloride, potassium chloride and ammonium chloride. The chloride ion concentration in the acid solution is 0.5 to 20 g / L, specifically, the chloride ion concentration in the acid solution is 1 to 18 g / L, and more specifically, the chloride ion concentration in the acid solution is 3 to 15 g / L; the concentration of chloride ions is to ensure that the water-soluble chloride salt is completely dissolved without solid precipitation.
[0038] The present application then performs a single-stage ion exchange on the chloride-containing reaction solution obtained above to achieve gallium-iron separation and obtain a gallium-loaded organic phase; the single-stage ion exchange resin includes one or more of polyurethane, tributyl phosphate leaching resin (CL-TBP), tributyl phosphate-n-heptane (TBP-nC7H16) and LSC-900. For example, the volume ratio of the ion exchange resin to the gallium-rich solution is 0.01-1. More specifically, the volume ratio of the content of the ion exchange resin to the gallium-rich solution after the reaction is 0.2-1:1. The specific method of the single-stage ion exchange is not limited to laboratory equipment, ion exchange towers, and ion exchange columns. The residual liquid of the single-stage ion exchange is used to produce iron salts. After cleaning, the gallium-loaded ion exchange resin is specifically cleaned with 4-6N HCl to remove impurities therein. The cleaning can be performed by stirring, shaking, ion exchange towers, ion exchange columns and other devices. The number of cleanings should be controlled at 1 to 3 times, and the washing water can be directly returned as a leaching agent for acid leaching.
[0039] After the above treatment, the gallium-loaded organic phase contains a very small amount of impurities in addition to gallium and zinc. Desorption is continued, and cleaning is performed after desorption. In order to obtain a gallium-based alloy with higher purity, the first desorption-first cleaning-second desorption-second cleaning-third desorption is preferably performed in this application, and finally three desorption liquids are collected, and solid-liquid separation is performed after adjusting the pH. The pH of the medium for the first desorption should be controlled at 5-9. For example, it can be selected from weak acid, weak base or neutral salt aqueous solution. More specifically, the medium for the first desorption includes one of dilute sulfuric acid solution, acetic acid solution, dilute hydrochloric acid solution and sodium hydroxide solution; a gallium-rich aqueous phase is obtained after the first desorption. The first cleaning is used to wash away impurities therein to obtain a gallium-loaded organic phase with slightly less impurities. The pH of the medium for the second desorption should be controlled at 5-9. For example, it can be selected from weak acid, weak base or neutral salt aqueous solution. More specifically, the medium for the second desorption includes one of dilute sulfuric acid solution, acetic acid solution, dilute hydrochloric acid solution and sodium hydroxide solution; a gallium-rich aqueous phase is obtained after the second desorption. The second washing is to wash away the impurities therein and obtain a gallium-loaded organic phase with slightly less impurities. The pH of the medium for the third desorption should be controlled at 5-9. For example, it can be selected from weak acid, weak base or neutral salt aqueous solution. More specifically, the medium for the third desorption includes one of dilute sulfuric acid solution, acetic acid solution, dilute hydrochloric acid solution and sodium hydroxide solution; after the third desorption, a gallium-rich aqueous phase is obtained. The third washing is to wash away the impurities therein and obtain a gallium-loaded organic phase with slightly less impurities. The desorption medium for the first desorption, the second desorption and the third desorption can be the same or different, and this application does not impose any special restrictions on this. Similarly, the cleaning agents for the first and second washings can be the same or different, and this application does not impose any special restrictions on this. The above three elutions, impurity removal and desorption make the gallium purity higher, and are a gallium enrichment process. After the third desorption, the three desorption liquids are collected, the pH is adjusted to 3.5-6, and then solid-liquid separation is performed. The obtained solid phase is alkali-dissolved to remove all the iron in the solid phase, and gallium-rich hydroxide is obtained after solid-liquid separation. The alkaline dissolving agent can be a strong alkaline solution such as sodium hydroxide and potassium hydroxide. The above ion exchange-elution step has a great influence on the purity of gallium. Less resin means less zinc co-extraction and lower final zinc content; and fewer elution times means higher subsequent zinc content.
[0040] The present application finally electrolyzes the solution obtained by solid-liquid separation to obtain a high-purity gallium-based liquid alloy. The anode material of the electrolysis includes graphite, platinum, stainless steel, lead, silver, titanium alloy, tungsten or molybdenum, and the cathode material includes copper-indium alloy, indium-gallium alloy or stainless steel. The electrolysis temperature is 10-100°C and the current density is 30-1000A / cm 2 Specifically, the electrolysis temperature is 30-90°C and the current density is 100-800A / cm 2More specifically, the electrolysis temperature is 40-70°C and the current density is 200-600A / cm 2 In the present application, the voltage and current of the electrolysis vary with different types of electrodes. The electrolysis can be either single-stage or multi-stage, depending on the concentration of gallium after alkali dissolution, electrode selection, and current density.
[0041] According to the needs of technical personnel in this field for gallium-based liquid metal products, technical personnel in this field can directly add one or more of gallium, zinc, tin and indium to the above-mentioned methyl liquid alloy to obtain gallium-based liquid metal products that comply with the national standard "GB / T39859-2021".
[0042] The present application provides a method for preparing gallium-based liquid metal, which directly synthesizes gallium-zinc alloy by using gallium-containing waste, realizes the recycling of waste, and the prepared gallium-based liquid metal has high gallium content, short gallium extraction process, good impurity removal effect, and also produces by-products with economic value; the prepared gallium-based liquid metal contains gallium ≥95wt%, zinc 1-5wt%, and the yield of gallium and zinc in the whole process is 85-95%.
[0043] In order to further understand the present invention, the preparation method of the gallium-based liquid metal provided by the present invention is described in detail below in conjunction with examples, and the protection scope of the present invention is not limited by the following examples.
[0044] Example 1
[0045] The present invention relates to a gallium-based liquid metal preparation method. The raw material of the vanadium-extracting converter dust mainly comprises 89wt% of iron oxide, 1wt% of ZnO, and the rest is a mixture of Na2O, MgO, CaCO3, Al2O3, TiO2, V2O5, Cr2O3, MnO, PbO, CuO, NiO, chlorides, sulfides, etc., with a total amount less than 10wt%. The gallium content in the raw material is 200g / t (the percentage is 0.002wt%), and the total amount of the above mixture and gallium is 10wt%.
[0046] Step 1: Leaching the raw material, the leaching agent is sulfuric acid; the leaching agent concentration is 50g / L, the leaching time is 0.5 hours, the stirring rate is 500rpm, the leaching temperature is 5°C, the liquid-solid ratio is 10, and three stages of acid leaching are adopted during the leaching process to reduce the acid consumption;
[0047] The second step is to add reduced iron powder to the leachate after the leaching is completed, with the molar Fe (raw material): molar Fe (reduced iron powder) being 0.5, and slowly add the reduced iron powder until the leachate has no color change after thiocyanate detection; during the process of adding the reduced iron powder, stirring and heating can be performed to accelerate the reaction rate of the reduced iron powder with the trivalent iron in the leachate;
[0048] The third step is to perform solid-liquid separation after the leaching solution has no color change after thiocyanate detection, and the residue is separated by suction filtration; a saturated NaOH solution is added to the separated solution to adjust the pH to 3.5, and solid-liquid separation is performed again. At this time, the liquid of the solid-liquid separation is a ferrous chloride solution, and the gallium content in the solid is about 0.2wt%, and the zinc content is 6wt%. The solid obtained above is acid-dissolved again, and the gallium content in the acid solution is 300ppm and the zinc content is 3g / L;
[0049] Step 4: Add 0.5 g / L sodium chloride to the acid solution to ensure that all water-soluble substances are dissolved without solid precipitation;
[0050] The fifth step is to perform single-stage ion exchange on the reaction solution obtained in the fourth step, wherein the ion exchange resin is polyurethane, and the volume ratio of the amount used to the reaction solution is 0.5; the ion exchange column is equipment, and the raffinate is used to produce iron salt;
[0051] Step 6: Use 4N HCl to wash the gallium-rich resin. When washing the resin, use a resin tower to wash the resin for 3 times. The washing water can be directly returned to leaching the raw material.
[0052] Step 7: Desorb the washed organic phase for the first time, and the desorption medium is a dilute sulfuric acid solution with a pH of 5;
[0053] Step 8: Use 4N HCl to wash the loaded resin again. The washing is carried out by vibration, and the washing water can be directly returned to leaching the raw materials;
[0054] Step 9, the washed loaded resin is desorbed for the second time, and the desorption medium is a dilute hydrochloric acid solution with a pH of 5;
[0055] Step 10: Use 6N HCl to wash the organic phase again. The washing is carried out through an ion exchange column, and the washing water can be directly returned to leach the raw materials;
[0056] Step 11, the washed organic phase is desorbed for the third time, and the desorption medium is a sodium hydroxide solution with a pH of 9;
[0057] Step 12: Collect the desorption liquid three times, adjust the pH to 6 and then perform solid-liquid separation;
[0058] The thirteenth step is to perform alkali dissolution on the solid after the solid-liquid separation in the twelfth step, wherein the alkali dissolution medium is a sodium hydroxide solution, and then perform solid-liquid separation again after the alkali dissolution;
[0059] The fourteenth step is to electrolyze the alkali-dissolved solution. During the electrolysis process, the anode material is graphite, the cathode is stainless steel, the electrolysis temperature is 90°C, and the current density is 1000A / m 2The electrolysis process is a primary electrolysis process; the primary product liquid alloy containing gallium is 99wt% and zinc is close to 1wt%, and the sum of other elements is less than 0.05wt%; the yield of gallium and zinc in the whole process is 95%;
[0060] In the fifteenth step, a certain amount of high-purity zinc is directly added to the primary liquid alloy to obtain the gallium-based liquid metal product LMG-5 that meets the national standard "GB / T39859-2021".
[0061] Example 2
[0062] The present invention relates to a gallium-based liquid metal preparation method, wherein the raw material vanadium extraction converter dust mainly comprises 95wt% iron oxide, 2wt% SiO2, 2wt% ZnO, and the rest is a mixture of Na2O, MgO, CaCO3, Al2O3, TiO2, V2O5, Cr2O3, MnO, PbO, CuO, NiO, chlorides, sulfides, etc., with a total amount less than 1wt%, the gallium content in the raw material is 600g / t (the percentage content is 0.006wt%), and the total amount of the above mixture and gallium is 1wt%;
[0063] The first step is to carry out acid leaching on the raw material, the leaching agent is a mixture of nitric acid and phosphoric acid, the leaching agent concentration is 500g / L, the leaching time is 6 hours, no stirring, the leaching temperature is 90°C, the liquid-solid ratio is 0.1, and 10 stages of acid leaching are adopted during the leaching process (the parameters of the 10 stages of acid leaching are as described above, the liquid-solid ratio is very small, and continuous leaching is required to reduce the acid consumption), thereby reducing the acid consumption;
[0064] In the second step, after the leaching is completed, reduced iron powder is added to the leaching solution, molar Fe (原料) : molar Fe (还原铁粉) The ratio of the reduced iron powder to the iodine concentration is 1.1, and the reduced iron powder is slowly added until the leaching solution has no color change after the thiocyanate detection. During the addition of the reduced iron powder, the mixture can be stirred to accelerate the reaction rate between the reduced iron powder and the trivalent iron in the leaching solution.
[0065] The third step is to perform solid-liquid separation after the leaching solution is tested for no color change by thiocyanate, and the residue is separated by filtering the leaching solution; a saturated NaOH solution is added to the separated solution to adjust the pH to 4.0, and solid-liquid separation is performed again. At this time, the liquid of the solid-liquid separation is a ferrous chloride solution, and the gallium content in the solid is about 0.25wt%, and the zinc content is 7wt%. The solid obtained above is acid-dissolved again, and the gallium content in the acid solution is 300ppm and the zinc content is 3.2g / L;
[0066] The fourth step is to add potassium chloride to the acid solution. After adding, the chloride ion concentration in the leachate is 20 g / L, ensuring that all water-soluble substances are dissolved without solid precipitation.
[0067] The fifth step is to perform single-stage ion exchange on the reaction solution obtained in the fourth step, wherein the ion exchange resin is a mixture of tributyl phosphate leaching resin (CL-TBP) and LSC-900, and the volume ratio of the amount used to the reaction solution is 0.02, and the remaining liquid is used to produce iron salt;
[0068] Step 6: Use 6N HCl to wash the gallium-rich resin. The resin tower is used for washing. The resin is washed three times. The washing water can be directly returned to leach the raw materials.
[0069] Step 7: Desorb the washed organic phase for the first time, using sodium bicarbonate solution as the desorption medium with a pH of 9;
[0070] Step 8: Use 6N HCl to wash the resin again. The resin is washed by vibration, and the washing water can be directly returned to leaching the raw materials;
[0071] Step 9: Desorb the cleaned resin for the second time, using sodium carbonate solution as the desorption medium with a pH of 9;
[0072] Step 10: Use 4N HCl to wash the resin again. The resin is washed through a resin tower, and the washing water can be directly returned to leaching the raw material;
[0073] Step 11, the cleaned resin is desorbed for the third time, and the desorption medium is an acetic acid solution with a pH of 5;
[0074] Step 12: Collect the desorption liquid three times, adjust the pH to 3.5 and then perform solid-liquid separation;
[0075] Step 13, alkali dissolving the solid after solid-liquid separation in step 12, wherein the alkali dissolving is potassium hydroxide solution, and solid-liquid separation is performed again after alkali dissolution;
[0076] The fourteenth step is to electrolyze the alkali-dissolved solution. During the electrolysis process, the anode material is stainless steel and the cathode is copper-indium alloy. The electrolysis temperature can be controlled at 10°C and the current density is 30A / m 2 The electrolysis process is a two-stage electrolysis process; the primary product liquid alloy containing gallium is 95wt%, zinc is slightly less than 5wt%, and the sum of other elements is less than 0.05wt%; the yield of gallium and zinc in the whole process is 85%;
[0077] In the fifteenth step, a small amount of gallium is directly added to the initial product produced by electrolysis to obtain the gallium-based liquid metal product LMG-5 that meets the national standard "GB / T39859-2021".
[0078] Comparative Example 1
[0079] The present invention relates to a gallium-based liquid metal preparation method. The raw material of the vanadium-extracting converter dust mainly comprises 89wt% of iron oxide, 1wt% of ZnO, and the rest is a mixture of Na2O, MgO, CaCO3, Al2O3, TiO2, V2O5, Cr2O3, MnO, PbO, CuO, NiO, chlorides, sulfides, etc., with a total amount less than 10wt%. The gallium content in the raw material is 200g / t (the percentage is 0.002wt%), and the total amount of the above mixture and gallium is 10wt%.
[0080] Step 1: Leaching the raw material, the leaching agent is sulfuric acid; the leaching agent concentration is 50g / L, the leaching time is 0.5 hours, the stirring rate is 500rpm, the leaching temperature is 5°C, the liquid-solid ratio is 10, and three stages of acid leaching are adopted during the leaching process to reduce the acid consumption;
[0081] The second step is to add reduced iron powder to the leachate after the leaching is completed, with the molar Fe (raw material): molar Fe (reduced iron powder) being 0.5, and slowly add the reduced iron powder until the leachate has no color change after thiocyanate detection; during the process of adding the reduced iron powder, stirring and heating can be performed to accelerate the reaction rate of the reduced iron powder with the trivalent iron in the leachate;
[0082] The third step is to perform solid-liquid separation after the leaching solution has no color change after thiocyanate detection, and the residue is separated by suction filtration; a saturated NaOH solution is added to the separated solution to adjust the pH to 6, and solid-liquid separation is performed again. At this time, the liquid of the solid-liquid separation is a ferrous chloride solution, and the gallium content in the solid is about 0.05wt%, and the zinc content is 3wt%. The solid obtained above is acid-dissolved again, and the gallium content in the solution is 150ppm and the zinc content is 2g / L;
[0083] Step 4: Add 0.5 g / L sodium chloride to the leachate to ensure that all water-soluble substances are dissolved without solid precipitation;
[0084] The fifth step is to perform single-stage ion exchange on the reaction solution obtained in the fourth step, wherein the ion exchange resin is polyurethane, and the volume ratio of the amount used to the reaction solution is 0.5; the ion exchange column is equipment, and the raffinate is used to produce iron salt;
[0085] Step 6: Use 4N HCl to wash the gallium-rich resin once. When washing the resin, use the resin tower to wash the resin three times. The washing water can be directly returned to leaching the raw materials.
[0086] Step 7: Desorb the washed organic phase for the first time, and the desorption medium is a dilute sulfuric acid solution with a pH of 5;
[0087] Step 8: Use 4N HCl to wash the loaded resin again. The washing is carried out by vibration, and the washing water can be directly returned to leaching the raw materials;
[0088] Step 9, the washed loaded resin is desorbed for the second time, and the desorption medium is a dilute hydrochloric acid solution with a pH of 5;
[0089] Step 10: Use 6N HCl to wash the organic phase again. The washing is carried out through an ion exchange column, and the washing water can be directly returned to leach the raw materials;
[0090] Step 11, the washed organic phase is desorbed for the third time, and the desorption medium is a sodium hydroxide solution with a pH of 9;
[0091] Step 12: Collect the desorption liquid three times, adjust the pH to 6 and then perform solid-liquid separation;
[0092] The thirteenth step is to perform alkali dissolution on the solid after the solid-liquid separation in the twelfth step, wherein the alkali dissolution medium is a sodium hydroxide solution, and then perform solid-liquid separation again after the alkali dissolution;
[0093] The fourteenth step is to electrolyze the alkali-dissolved solution. During the electrolysis process, the anode material is graphite, the cathode is stainless steel, the electrolysis temperature is 90°C, and the current density is 1000A / m 2 The electrolysis process is a primary electrolysis; since the pH is not controlled at 2-5 during the preparation of the gallium-rich material, the iron content in the obtained gallium-rich material is relatively high. In the subsequent impurity removal process, the existing process is not thorough in impurity removal, and the addition of other low-melting-point metals cannot meet the gallium-based liquid metal products of GB / T 39859-2021.
[0094] Comparative Example 2
[0095] The present invention relates to a gallium-based liquid metal preparation method, wherein the raw material vanadium extraction converter dust mainly comprises 95wt% iron oxide, 2wt% SiO2, 2wt% ZnO, and the rest is a mixture of Na2O, MgO, CaCO3, Al2O3, TiO2, V2O5, Cr2O3, MnO, PbO, CuO, NiO, chlorides, sulfides, etc., with a total amount less than 1wt%, the gallium content in the raw material is 600g / t (the percentage content is 0.006wt%), and the total amount of the above mixture and gallium is 1wt%;
[0096] The first step is to carry out acid leaching on the raw material, the leaching agent is a mixture of nitric acid and phosphoric acid, the leaching agent concentration is 500g / L, the leaching time is 6 hours, no stirring, the leaching temperature is 90°C, the liquid-solid ratio is 0.1, and 10 stages of acid leaching are adopted during the leaching process (the parameters of the 10 stages of acid leaching are as described above, the liquid-solid ratio is very small, and continuous leaching is required to reduce the acid consumption), thereby reducing the acid consumption;
[0097] In the second step, after the leaching is completed, reduced iron powder is added to the leaching solution, molar Fe (原料) : molar Fe(还原铁粉) The ratio of the reduced iron powder to the iodine concentration is 1.1, and the reduced iron powder is slowly added until the leaching solution has no color change after the thiocyanate detection. During the addition of the reduced iron powder, the mixture can be stirred to accelerate the reaction rate between the reduced iron powder and the trivalent iron in the leaching solution.
[0098] The third step is to perform solid-liquid separation after the leaching solution has no color change after thiocyanate detection, and the residue is separated by filtering the leaching solution; the pH is adjusted to 4 using a saturated NaOH solution, and solid-liquid separation is performed again. At this time, the liquid for solid-liquid separation is a ferrous chloride solution, and the gallium content in the solid is about 0.3wt%, and the zinc content is 7wt%. The solid obtained above is acid-dissolved again, and the gallium content in the acid solution is 400ppm and the zinc content is 3.5g / L;
[0099] The fourth step is to add potassium chloride to the acid solution. After adding, the chloride ion concentration in the leachate is 20 g / L, ensuring that all water-soluble substances are dissolved without solid precipitation.
[0100] The fifth step is to subject the reaction liquid obtained in the fourth step to single-stage centrifugal extraction, wherein the effective extractant is P507, the diluent is a mixture of sulfonated kerosene and aviation kerosene, the effective extractant is 30% of the total volume of the effective extractant and the diluent, and the raffinate is used to produce iron salt;
[0101] The sixth step is to wash the organic phase with 6N HCl. The organic phase is washed by a centrifugal extraction device for 3 times. The washing water can be directly returned to leach the raw materials.
[0102] Step 7: The washed organic phase is stripped for the first time, with sodium bicarbonate solution as the stripping medium at a pH of 9;
[0103] Step 8: Wash the organic phase again with 6N HCl. The washing of the organic phase is performed by vibration, and the washing water can be directly returned to leach the raw materials.
[0104] Step 9, the washed organic phase is stripped for the second time, with sodium carbonate solution as the stripping medium and a pH of 9;
[0105] Step 10, washing the organic phase again with 4N HCl, the washing of the organic phase is carried out through an extraction tower, and the washing water can be directly returned to leach the raw materials;
[0106] Step 11, the washed organic phase is stripped for the third time, and the stripping medium is an acetic acid solution with a pH of 5;
[0107] Step 12, collecting three stripping solutions, adjusting the pH to 3.5 and then performing solid-liquid separation;
[0108] Step 13, alkali dissolving the solid after solid-liquid separation in step 12, wherein the alkali dissolving is potassium hydroxide solution, and solid-liquid separation is performed again after alkali dissolution;
[0109] When the acidity of the leaching solution is high, the gallium recovery rate using the single-stage extraction method is low and does not meet the requirements of electrolysis. Therefore, a gallium-based liquid metal product that meets the national standard "GB / T 39859-2021" cannot be obtained.
[0110] The above embodiments are only used to help understand the method and core idea of the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.
[0111] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing gallium-based liquid metal, comprising the following steps: S1) acid leaching gallium-containing waste to obtain an acidic leaching solution; the gallium-containing waste comprises 89-95wt% Fe oxide, 0-2wt% Si, 1-5wt% ZnO, and 200-600g / t Ga; S2) mixing the acidic leachate and iron powder, performing solid-liquid separation after the reaction, and obtaining a gallium-containing leachate; adjusting the pH to 2-5 using a saturated NaOH solution, and performing solid-liquid separation again; and acid-dissolving the solid obtained by the solid-liquid separation again to obtain an acid solution; S3) adding a water-soluble chloride salt to the acid solution, performing a single-stage ion exchange after the reaction to obtain a gallium-loaded ion exchange resin, and washing the ion exchange resin; S4) performing a first desorption on the ion exchange resin washed in step S3), and performing a first washing on the ion exchange resin obtained by the first desorption; S5) adjusting the pH of the liquid obtained in step S4) and performing solid-liquid separation, dissolving the obtained solid in alkali, and performing solid-liquid separation again; S6) electrolyzing the liquid phase obtained in step S5) to obtain a gallium-based liquid metal; the gallium-based liquid metal contains ≥95wt% gallium and 1-5wt% zinc.
2. The preparation method according to claim 1, characterized in that: Step S4) also includes a second desorption and a third desorption, specifically: performing a first desorption on the ion exchange resin after washing in step S3), and performing a first washing on the ion exchange resin obtained by the first desorption; Desorbing the ion exchange resin after the first washing for a second time, and washing the obtained ion exchange resin for a second time; The ion exchange resin after the second washing is subjected to a third desorption.
3. The preparation method according to claim 1 or 2, characterized in that: Step S6) also includes: One or more of gallium, zinc, indium and tin are added to the obtained gallium-based liquid metal.
4. The preparation method according to claim 3, characterized in that: In step S1), the leaching agent of the acid leaching includes one or more of sulfuric acid, oxalic acid, nitric acid and phosphoric acid, the concentration of the leaching agent is 50-500 g / L, the time of the acid leaching is 0.5-6 h, the temperature is 5-100° C., and the liquid-to-solid ratio of the acid leaching is (10-0.1):
1.
5. The preparation method according to claim 3, characterized in that: In step S2), the ratio of the molar amount of iron in the leaching solution to the molar amount of iron powder is (0.5-1.5):1; the solid-liquid separation method is suction filtration, filter pressing or centrifugation.
6. The preparation method according to claim 3, characterized in that: In step S3), the water-soluble chloride salt includes one or more of sodium chloride, potassium chloride and ammonium chloride, and the chloride ion concentration of the water-soluble chloride salt in the gallium-containing leaching solution is 0.5-20 g / L.
7. The preparation method according to claim 1, characterized in that: In step S3), the ion exchange resin of the single-stage ion exchange includes one or more of polyurethane, tributyl phosphate leaching resin, tributyl phosphate-n-heptane and LSC-900, and the volume ratio of the ion exchange resin to the gallium-rich solution after the reaction is 0.01-1.
8. The preparation method according to claim 3, characterized in that: The pH of the desorption medium of the first desorption is 5-9, and the desorption medium includes one of a dilute sulfuric acid solution, an acetic acid solution, a dilute hydrochloric acid solution and a sodium hydroxide solution.
9. The preparation method according to claim 3, characterized in that: In step S5), the pH is adjusted to 3.5-6, and the alkali-soluble reagent includes potassium hydroxide or sodium hydroxide.
10. The preparation method according to claim 3, characterized in that: The anode material of the electrolysis includes graphite, platinum, stainless steel, lead, silver, titanium alloy, tungsten or molybdenum, the cathode material includes copper indium alloy, indium gallium alloy or stainless steel, the electrolysis temperature is 10-100°C, the current density is 30-1000A / cm 2 .