Diamond-containing composite material, preparation method and application

By wrapping Ni-Fe-Sn-Cu prealloy powder on the diamond drill bit and performing mixing treatment, a close connection between the protective layer and the alloy layer is solved, and the problem of insufficient aging and life of the diamond drill bit in the prior art is achieved. High wear resistance and longer service life.

CN118880116AActive Publication Date: 2024-11-01GUANGDONG TECHN COLLEGE OF WATER RESOURCES & ELECTRIC ENG
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410912615.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-11-01
Estimated Expiration
2044-07-09

AI Technical Summary

Technical Problem

The aging and lifespan of existing diamond drill bits is insufficient and further optimization is needed.

Method used

The diamond is wrapped with Ni-Fe-Sn-Cu pre-alloy powder and then mixed to form a close connection between the porous protective layer and the alloy layer, improving the wear resistance and drillable depth of the drill bit.

Benefits of technology

It significantly improves the aging and life of diamond drill bits, extends service life, and improves the overall drillable depth of the drill bit.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention belongs to the field of new materials, and discloses a preparation method of a diamond-containing composite material, which comprises the following steps: step 1, mixing Ni-Fe-Sn-Cu pre-alloyed powder, a polymer binder and diamond; 2, curing the mixture in the step 1, and then crushing the cured product into particles capable of passing through a 30-mesh screen; 3, heating in an oxygen or air atmosphere to carbonize and oxidize the polymer binder in the particles obtained in the step 2; then heating in a reducing gas atmosphere to reduce the oxidized metal to obtain diamond particles; the surfaces of the diamond particles are covered with a layer of porous Ni-Fe-Sn-Cu pre-alloyed powder surface layer; 4, the Cr-Fe pre-alloyed powder, the Ni-Fe-Sn-Cu pre-alloyed powder, the Cr-Ni-Fe pre-alloyed powder, the metal binding agent and the diamond particles are mixed; 5, the mixture obtained in the step 4 is subjected to cold press molding, sintering and hot pressing, and the composite material is obtained. According to the composite material, the Ni-Fe-Sn-Cu pre-alloyed powder is firstly adopted to wrap the diamond, and then the prior patent technology is adopted to carry out subsequent mixing treatment, so that the aging of the obtained composite material is improved, and the service life of the obtained composite material is prolonged. The invention also provides a preparation method and application of the composite material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of new materials, in particular to a composite material containing diamond, a preparation method and application thereof. Background Art

[0002] The applicant has previously filed an invention patent application: CN117047109A, a diamond-impregnated drill bit and a preparation method thereof, the method uses 30-45 parts of skeleton material, 10-20 parts of intermediate components, 45-60 parts of bonding materials and 15-19 parts of diamond to prepare a composite material, wherein the skeleton material includes Cr-Fe pre-alloyed powder, Ni-Fe-Sn-Cu pre-alloyed powder and Cr-Ni-Fe pre-alloyed powder. Its performance is an average aging of 6-7m / h and an average life of 45-57m.

[0003] After further research, the applicant found that the above performance can be further optimized.

[0004] The technical problem to be solved by this scheme is: how to improve the effectiveness and life of diamond drill bits. Summary of the invention

[0005] The purpose of the present invention is to provide a composite material containing diamond, wherein the composite material is firstly coated with Ni-Fe-Sn-Cu pre-alloyed powder, and then the composite material is subsequently mixed using the prior patented technology, so that the aging and life of the composite material are improved.

[0006] The invention also provides a preparation method and application of the composite material.

[0007] To achieve the above object, the present invention provides the following technical solutions:

[0008] A method for preparing a composite material containing diamond comprises the following steps:

[0009] Step 1: Mix Ni-Fe-Sn-Cu pre-alloy powder, polymer binder and diamond;

[0010] Step 2: solidify the mixture of step 1, and then crush the solidified product into particles that can pass through a 30-mesh sieve;

[0011] Step 3: heating in an oxygen or air atmosphere to carbonize and oxidize the polymer binder in the particles obtained in step 2; then heating in a reducing gas atmosphere to reduce the oxidized metal to obtain diamond particles; the surface of the diamond particles is covered with a porous Ni-Fe-Sn-Cu pre-alloyed powder surface layer;

[0012] Step 4: Mixing Cr-Fe pre-alloyed powder, Ni-Fe-Sn-Cu pre-alloyed powder, Cr-Ni-Fe pre-alloyed powder, metal binder and diamond particles;

[0013] Step 5: The mixture obtained in step 4 is subjected to cold pressing, sintering and hot pressing to obtain the composite material.

[0014] The core innovation of the present invention is that the diamond is firstly wrapped with Ni-Fe-Sn-Cu pre-alloyed powder, and then the prior patented technology is used for subsequent mixing treatment, so that the aging and life of the obtained composite material are improved.

[0015] The specific principle is: Existing research shows that Ni-Sn-Cu pre-alloyed powder has good wear resistance; when a small amount of iron is added, its plasticity is significantly improved. Compared with Cr-Fe pre-alloyed powder and Cr-Ni-Fe pre-alloyed powder, the biggest advantage of Ni-Fe-Sn-Cu pre-alloyed powder is its good plasticity.

[0016] When diamond is wrapped with Ni-Fe-Sn-Cu pre-alloyed powder, it is equivalent to embedding a protective layer on the surface of the diamond, similar to the setting of a diamond ring. This protective layer and the subsequent alloy layer can be fully combined after hot pressing. When the diamond is rubbed and scratched, this protective layer can form a tight connection with the alloy layer, making full use of the plasticity and wear resistance of the Ni-Fe-Sn-Cu alloy, so that the diamond is not easily pulled out of the alloy layer. The shedding of diamond is accompanied by the wear of the alloy layer, which can effectively improve the life of the drill bit. At the same time, the alloy formed by Cr-Fe pre-alloyed powder, Ni-Fe-Sn-Cu pre-alloyed powder, and Cr-Ni-Fe pre-alloyed powder has good wear resistance and can effectively improve the overall drilling depth of the drill bit.

[0017] In the above-mentioned method for preparing a composite material containing diamond, the polymer binder is an epoxy resin binder;

[0018] The weight ratio of the Ni-Fe-Sn-Cu pre-alloy powder, the polymer binder and the diamond is 1-2:0.05-0.2:1.

[0019] In the above-mentioned method for preparing the composite material containing diamond, the fineness of the diamond is 40-55 meshes.

[0020] In the above-mentioned method for preparing the composite material containing diamond, the fineness of the Ni-Fe-Sn-Cu pre-alloyed powder, the Cr-Fe pre-alloyed powder, the Cr-Ni-Fe pre-alloyed powder and the metal binder are all 200-300 meshes.

[0021] In the above-mentioned method for preparing a composite material containing diamond, in the step 3, the heating temperature in an oxygen or air atmosphere is 330-420° C.;

[0022] The heating temperature is 600-700°C in a reducing gas atmosphere;

[0023] Heat at 330-420℃ for 1-3h; heat at 600-700℃ for 3-4h.

[0024] In the above-mentioned method for preparing the diamond-containing composite material, the molar ratio of Cr to Fe in the Cr-Fe pre-alloyed powder is 1:0.5; the molar ratio of Ni, Fe, Sn, and Cu in the Ni-Fe-Sn-Cu pre-alloyed powder is 15:0.2:7:1; and the molar ratio of Cr, Ni, and Fe in the Cr-Ni-Fe pre-alloyed powder is 6:10:3.

[0025] In the above-mentioned method for preparing the diamond-containing composite material, in step 4, the ratio of Cr-Fe pre-alloyed powder, Ni-Fe-Sn-Cu pre-alloyed powder, Cr-Ni-Fe pre-alloyed powder, metal binder, and diamond particles is: 5-6:15-20:15-20:40-50:25-35.

[0026] In the above-mentioned method for preparing the composite material containing diamond, in the step 4, Co powder and Ni powder are further added; the weight ratio of the Cr-Fe pre-alloyed powder, Co powder and Ni powder is 5-6:5-10:5-10.

[0027] At the same time, the present invention also discloses a composite material containing diamond, which is prepared by any of the above methods.

[0028] Finally, the present invention also discloses the use of the composite material as described above to prepare a drill bit.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] The composite material of the invention firstly uses Ni-Fe-Sn-Cu pre-alloyed powder to wrap diamond, and then uses the prior patented technology to perform subsequent material mixing treatment, so that the aging and life of the obtained composite material are improved. DETAILED DESCRIPTION

[0031] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] Example 1

[0033] A method for preparing a composite material containing diamond comprises the following steps:

[0034] Step 1: Mix Ni-Fe-Sn-Cu pre-alloy powder, polymer binder and diamond;

[0035] The weight ratio of Ni-Fe-Sn-Cu pre-alloyed powder, polymer binder, and diamond is 1:0.1:1;

[0036] The particle size of diamond is through a 50-mesh screen; the chemical formula of Ni-Fe-Sn-Cu pre-alloyed powder is 15Ni-0.2Fe-7Sn-Cu;

[0037] The polymer binder is bisphenol A epoxy resin, which contains a curing agent. After mixing, it can form a brittle solid structure.

[0038] Step 2: solidify the mixture of step 1, and then crush the solidified product into particles that can pass through a 30-mesh sieve;

[0039] Step 3: heating in an air atmosphere to carbonize and oxidize the polymer binder in the particles obtained in step 2;

[0040] The heating temperature is 400°C and the heating time is 3h;

[0041] Then, heating is performed in a hydrogen reducing gas atmosphere to reduce the oxidized metal to obtain diamond particles; the surface of the diamond particles is covered with a porous surface layer of Ni-Fe-Sn-Cu pre-alloyed powder;

[0042] The heating temperature is 600-700°C and the heating time is 3h.

[0043] Step 4: Mix Cr-Fe pre-alloyed powder, Ni-Fe-Sn-Cu pre-alloyed powder, Cr-Ni-Fe pre-alloyed powder, metal binder and diamond particles in a mixer for 70 minutes at a rotating speed of 30 r / min;

[0044] The chemical formula of Ni-Fe-Sn-Cu prealloy powder is the same as step 1; the chemical formula of Cr-Fe prealloy powder is Cr-0.5Fe; the chemical formula of Cr-Ni-Fe prealloy powder is 6Cr-10Ni-3Fe; the metal binder is 660-Cu;

[0045] The weight ratio of Cr-Fe pre-alloyed powder, Ni-Fe-Sn-Cu pre-alloyed powder, Cr-Ni-Fe pre-alloyed powder, metal binder and diamond particles is: 5.5:18:18:45:30;

[0046] Step 5: The mixture obtained in step 4 is subjected to cold pressing, sintering and hot pressing to obtain the composite material.

[0047] The sintering temperature of the sintering hot pressing process is 940°C, the hot pressing pressure is 50KN, the holding time is 6min, and the total time of the sintering hot pressing process is 10min.

[0048] Example 2

[0049] It is substantially the same as Example 1, except that the weight ratio of Cr-Fe pre-alloy powder, Ni-Fe-Sn-Cu pre-alloy powder, Cr-Ni-Fe pre-alloy powder, metal binder and diamond particles is 5:20:15:50:25.

[0050] Example 3

[0051] It is substantially the same as Example 1, except that the weight ratio of Cr-Fe pre-alloy powder, Ni-Fe-Sn-Cu pre-alloy powder, Cr-Ni-Fe pre-alloy powder, metal binder, and diamond particles is 6:15:20:40:35.

[0052] Example 4

[0053] The process is substantially the same as Example 1, except that Co powder and Ni powder are further added in step 4, and the weight ratio of Cr-Fe pre-alloy powder, Ni-Fe-Sn-Cu pre-alloy powder, Cr-Ni-Fe pre-alloy powder, metal binder, diamond particles, Co powder and Ni powder is 5.5:18:18:45:30:5:5.

[0054] Example 5

[0055] The process is substantially the same as Example 1, except that Co powder and Ni powder are further added in step 4, and the weight ratio of Cr-Fe pre-alloy powder, Ni-Fe-Sn-Cu pre-alloy powder, Cr-Ni-Fe pre-alloy powder, metal binder, diamond particles, Co powder and Ni powder is 5.5:18:18:45:30:10:10.

[0056] Comparative Example 1

[0057] A method for preparing a composite material containing diamond comprises the following steps:

[0058] Step 1: Mix Cr-Fe pre-alloyed powder, Ni-Fe-Sn-Cu pre-alloyed powder, Cr-Ni-Fe pre-alloyed powder, metal binder and diamond particles in a mixer for 70 minutes at a rotating speed of 30 r / min;

[0059] The diamond particles in this step are: diamonds without any covering layer on the surface passing through a 50-mesh sieve;

[0060] The proportions and chemical formulas of the above five materials are the same as those in Example 1.

[0061] Step 2: The mixture obtained in step 1 is subjected to cold pressing, sintering and hot pressing to obtain the composite material.

[0062] The sintering temperature of the sintering hot pressing process is 700°C, the hot pressing pressure is 50KN, the holding time is 6min, and the total time of the sintering hot pressing process is 10min.

[0063] Comparative Example 2

[0064] A method for preparing a composite material containing diamond comprises the following steps:

[0065] Step 1: Mix Cr-Fe pre-alloyed powder, Ni-Fe-Sn-Cu pre-alloyed powder, Cr-Ni-Fe pre-alloyed powder, metal binder, diamond particles, Co powder and Ni powder in a mixer for 70 minutes at a rotating speed of 30 r / min;

[0066] The diamond particles in this step are: diamonds without any covering layer on the surface passing through a 50-mesh sieve;

[0067] The proportions and chemical formulas of the above 7 materials are the same as those in Example 1.

[0068] Step 2: The mixture obtained in step 1 is subjected to cold pressing, sintering and hot pressing to obtain the composite material.

[0069] The sintering temperature of the sintering hot pressing process is 700°C, the hot pressing pressure is 50KN, the holding time is 6min, and the total time of the sintering hot pressing process is 10min.

[0070] Performance Testing

[0071] The composite materials of the above embodiment and comparative example were used to prepare diamond drill bits for testing, using a 100-meter core drilling double-tube drilling, a rotation speed of 600-900 r / min, and a concrete foundation with a concrete grade of C35. The aging and average life of the test were tested.

[0072] The test results can be found in Table 1;

[0073] Table 1 Test results

[0074]

[0075]

[0076] Result analysis:

[0077] 1. It can be seen from Examples 1-3 that the drill bit made of the composite material of the present invention has a long aging and service life;

[0078] 2. It can be seen from Examples 4 and 5 that, as described in the prior application of this case, adding a small amount of Co powder and Ni powder is helpful for the overall toughness of the alloy and can increase the service life of the drill bit.

[0079] 3. In Example 2 and Example 3, the increase or decrease of diamond particles can not achieve the best in terms of aging and service life. The possible reason is that the drilling efficiency is related to the amount of diamond. At the same time, too much diamond can increase the aging in theory, but the actual aging is reduced. The possible reason is that the increase in the amount of diamond reaches the reduction of the holding force of the alloy for the diamond particles, resulting in the diamond particles falling off when the alloy is not completely worn, thereby reducing the aging. The amount of diamond particles is too little, although the holding force increases, the wear rate is accelerated and the aging is also reduced.

[0080] 4. It can be seen from Comparative Examples 1 and 2 that the prior art of the applicant cannot achieve the effect of the present invention.

[0081] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations that fall within the meaning and scope of the equivalent elements of the claims be included in the invention. The claims should not be considered as limiting the claims to which they refer.

Claims

1. A method for preparing a multi-layer thin-wall drill bit, characterized in that: The steps include: Step 1: Mix Ni-Fe-Sn-Cu pre-alloy powder, polymer binder and diamond; Step 2: solidify the mixture of step 1, and then crush the solidified product into particles that can pass through a 30-mesh sieve; Step 3: heating in an oxygen or air atmosphere to carbonize and oxidize the polymer binder in the particles obtained in step 2; then heating in a reducing gas atmosphere to reduce the oxidized metal to obtain diamond particles; the surface of the diamond particles is covered with a porous Ni-Fe-Sn-Cu pre-alloyed powder surface layer; Step 4: Mixing Cr-Fe pre-alloyed powder, Ni-Fe-Sn-Cu pre-alloyed powder, Cr-Ni-Fe pre-alloyed powder, metal binder and diamond particles; Step 5: The mixture obtained in step 4 is subjected to cold pressing, sintering and hot pressing to obtain the composite material.

2. The method for preparing a composite material containing diamond according to claim 1, characterized in that: The polymer binder is an epoxy resin binder; The weight ratio of the Ni-Fe-Sn-Cu pre-alloy powder, the polymer binder and the diamond is 1-2:0.05-0.2:

1.

3. The method for preparing a composite material containing diamond according to claim 1, characterized in that: The fineness of the diamond is 40-55 meshes.

4. The method for preparing a composite material containing diamond according to claim 1, characterized in that: The fineness of the Ni-Fe-Sn-Cu pre-alloyed powder, the Cr-Fe pre-alloyed powder, the Cr-Ni-Fe pre-alloyed powder and the metal binder are all 200-300 meshes.

5. The method for preparing a composite material containing diamond according to claim 1, characterized in that: In step 3, the heating temperature in the oxygen or air atmosphere is 330-420° C.; The heating temperature is 600-700°C in a reducing gas atmosphere; Heat at 330-420℃ for 1-3h; heat at 600-700℃ for 3-4h.

6. The method for preparing a composite material containing diamond according to claim 1, characterized in that: The molar ratio of Cr to Fe in the Cr-Fe pre-alloyed powder is 1:0.5; the molar ratio of Ni, Fe, Sn, and Cu in the Ni-Fe-Sn-Cu pre-alloyed powder is 15:0.2:7:1; and the molar ratio of Cr, Ni, and Fe in the Cr-Ni-Fe pre-alloyed powder is 6:10:

3.

7. The method for preparing a composite material containing diamond according to claim 1, characterized in that: In step 4, the ratio of Cr-Fe pre-alloyed powder, Ni-Fe-Sn-Cu pre-alloyed powder, Cr-Ni-Fe pre-alloyed powder, metal binder and diamond particles is 5-6:15-20:15-20:40-50:25-35.

8. The method for preparing a composite material containing diamond according to claim 7, characterized in that: In the step 4, Co powder and Ni powder are also added; the weight ratio of the Cr-Fe pre-alloyed powder, Co powder and Ni powder is 5-6:5-10:5-10.

9. A composite material containing diamond, characterized in that: The method is prepared by any one of claims 1 to 8.

10. Use of the composite material according to claim 9 in preparing a drill bit.

Citation Information

Patent Citations

  • Super hard alloy baseplate outer circumference cutting blade and manufacturing method thereof

    CN103459091A

  • Bonded abrasives formed by uniaxial hot pressing

    CN103826801A

  • Grinding wheel for roughing and thinning mobile phone backboard glass and preparation method of grinding wheel

    CN114378730A

  • High-entropy alloy-diamond superhard composite material with high self-sharpening and strong heat dissipation as well as preparation method and application of high-entropy alloy-diamond superhard composite material

    CN114921677A

  • Diamond-impregnated drill bit and preparation method thereof

    CN117047109A