Hard alloy containing components of WC, Co, Ni, Cr and Al and preparation method of hard alloy
By optimizing the sintering process parameters and vacuum heat treatment during the sintering process of WC-Co-Ni-Cr-Al cemented carbide, the pore defect problem caused by AlN cracking is solved, the denseness and strength of the material are improved, and the high stress conditions are adapted to demand.
Patent Information
- Application Number
- CN202410920560.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-07-10
AI Technical Summary
The cracking of AlN during the sintering process of WC-Co-Ni-Cr-Al cemented carbide leads to pore defects, affecting the density and mechanical properties of the material, and it is difficult to adapt to high-stress and high-strength working conditions.
By optimizing the sintering process parameters and combining the design of vacuum degree and temperature increase rate, the cracking and de-N treatment of AlN is completed in the solid phase sintering stage to ensure that AlN is completely cracked at a lower temperature, avoiding residual AlN entering the liquid phase sintering stage, and vacuum heat treatment is used Improve the density and performance of the alloy.
The densification of WC-Co-Ni-Cr-Al large single-weight cemented carbide is realized, which improves the performance stability and strength of the material, ensures the high-temperature oxidation resistance and wear resistance of the alloy, and is suitable for high-stress conditions. .
Smart Images

Figure CN118880146A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of cemented carbide, and more particularly to a cemented carbide containing WC, Co, Ni, Cr and Al components and a preparation method thereof. Background Art
[0002] Cemented carbide is mainly composed of refractory metal hard phase WC as the matrix and Co or Ni as the bonding phase. It is a high-hardness and high-wear-resistant material prepared by powder metallurgy. It plays an irreplaceable role in application fields such as cutting tools, impact tools and wear-resistant parts. It is one of the indispensable key hard materials in my country's high-end manufacturing industry and is given the reputation of "industrial teeth".
[0003] Cemented carbide roller ring is also a composite material prepared by powder metallurgy with refractory metal compounds as the skeleton and transition metals as the binder. Due to its high strength, high hardness, excellent wear resistance and high temperature resistance, it is widely used in the rolling production of bars, wires, special steels, rebars, etc. Compared with traditional cast iron roller rings, the steel rolling efficiency has been greatly improved.
[0004] The WC-Co cemented carbide roller ring used in the early days, although it has good stability and reliability, the temperature of its contact with red steel can be close to 80% of its liquidus eutectic temperature. The latest generation of cemented carbide roller rings for high-speed wires in advanced foreign companies generally use Co-Ni-Cr as a binder, such as the C10C, C15C, C20C, C25C, and C30T roller ring brands of Swedish Sandvik; the American sintered metal
[0005] The fourth generation SM-N series roller rings of SinterMet, LLC; CE260 of Luxembourg CERAMETAL. The roller rings of these advanced foreign companies are mainly improved by adding Ni and a small amount of Cr elements to improve the oxidation resistance and corrosion resistance of the bonding phase, which can make WC-Ni-Co-Cr have significantly higher wear resistance and high temperature oxidation resistance than WC-Co alloy under the condition of equivalent strength and hardness. The use of WC-Ni-Co-Cr cemented carbide roller rings can not only improve the surface quality of the rolled material, but also improve the high temperature stability and corrosion resistance of the roller ring, and its applicable working conditions are wider.
[0006] WC-Co-Ni-Cr cemented carbide has high hardness, strength and wear resistance, but in recent years, with the technological innovation and progress of downstream steel enterprises, traditional WC-Co-Ni-Cr cemented carbide is difficult to adapt to the harsh working conditions of high stress and high strength. The country attaches great importance to energy conservation and consumption reduction in the steel industry and encourages the steel industry to introduce new technologies. In 2018, the country implemented the new standard GB / T1499.2-2018 for steel bar enterprises to replace GB / T1499.2-2007. The rolling of rebar can no longer obtain high strength through strong water cooling to avoid the formation of closed martensite structure; at the same time, in order to reduce the amount and cost of alloy elements, the most feasible method is to adopt low-temperature rolling, which means rolling and producing rebar below the recrystallization temperature to avoid the growth of grains refined by rolling deformation, thereby reducing the content of alloy elements, improving the elongation and strength of the material, and will not produce closed martensite structure, meeting the requirements of the new national standard for steel performance and organizational structure.
[0007] With the advancement of steel rolling technology and environmental cost control, steel companies have stepped up their efforts to improve product competitiveness and technological upgrading, and low-temperature rolling technology has been valued and applied by various companies. The application of WC-Co-Ni-Cr-Al materials immediately appeared. The production and manufacturing of WC-Co-Ni-Cr-Al materials encountered certain difficulties. Although the addition of Al elements promoted the improvement of the mechanical properties of the alloy materials under high temperature conditions, the single Al element was relatively active and easily oxidized during the manufacturing process. In 1985, Japanese scholar Nishigaki proposed to use AlN instead of Al for addition at the 11th Plancy International Academic Conference, generating γ' phase (Ni, Co)3Al during the sintering process, so that the alloy has excellent toughness, wear resistance, high temperature strength and oxidation resistance, which theoretically solved this problem.
[0008] Patent CN201110449684.X discloses a WC-Co-Ni-Al-B cemented carbide roller ring material and a manufacturing method, which uses AlN to replace Al and adds a trace amount of B to improve the creep resistance, strength, hardness and wear resistance of the cemented carbide.
[0009] Related literature reports that AlN is very stable at room temperature and pressure. When AlN is used to replace Al in the production of WC-Co-Ni-Cr-Al cemented carbide roller rings, due to the large unit weight of the product (usually reaching more than 10kg), AlN will undergo different degrees of cracking during the sintering process, resulting in the appearance of Al oxides, thereby inducing the generation of pore defects. This has a serious impact on the compactness of the WC-Co-Ni-Cr-Al cemented carbide roller ring product and affects its mechanical properties. Summary of the invention
[0010] The purpose of the present invention is to provide a method for mass production of large single weight coarse-grained cemented carbide WC-Co-Ni-Cr-Al in view of the shortcomings and difficulties of the prior art. The cracking of AlN requires certain prerequisites, namely vacuum and temperature. The scheme is optimized and designed during the sintering stage, and AlN cracking and N removal treatment is performed. Compared with the prior art, this scheme mainly solves the following problems: 1) By optimizing the sintering process parameters, the compactness of the microstructure of the WC-Co-Ni-Cr-Al large single weight cemented carbide product is improved, thereby improving the performance stability of the product; 2) The strength and hardness of the cemented carbide are improved by vacuum heat treatment.
[0011] In order to achieve the above object, the present invention adopts the following technical solution:
[0012] A hard alloy containing WC, Co, Ni, Cr and Al, which comprises the following components by mass percentage: Co7.5-16%, Ni7.5-16%, Cr0.5-1.0%, AlN0.8-2.7%, and the balance is WC;
[0013] Among them, the mass ratio of Co to Ni is 1:1.
[0014] Preferably, the particle size of the AlN powder is ≤2 μm.
[0015] Another object of the present invention is to provide a method for preparing the above-mentioned cemented carbide containing WC, Co, Ni, Cr and Al components, comprising: wet-grinding and mixing AlN powder with coarse WC powder, Co powder, Ni powder and Cr powder / Cr carbide, ball-milling to a certain point, followed by drying, sieving, granulating and pressing into a green embryo, and then removing the molding agent, solid phase sintering, liquid phase sintering and vacuum heat treatment in sequence;
[0016] The solid phase sintering includes: a first stage of setting a heat preservation section at 700°C to 800°C, during which the vacuum is reduced to a limit of ≤5Pa; a second stage of heating at (700-800)°C to 1000°C; a third stage of heating at 1000°C to 1250°C; a fourth stage of heating at 1250°C to 1290°C; and a fifth stage of heating at 1290°C to 1320°C;
[0017] The vacuum degree in the five solid-phase sintering stages was monitored and named P1, P2, P3, P4 and P5, respectively, where P1 took the minimum value and P2-P5 took the maximum value;
[0018] Comparison is performed based on the minimum value of P1. When P4≤P1, P4<P3, and P5<P4 are satisfied at the same time, it is judged that the cracking of AlN during the sintering process of WC-Co-Ni-Cr-Al material has been completed, and liquid phase sintering is directly entered; (To achieve the above conditions, the heating rates of the P3, P4, and P5 stages can be adjusted and matched, and the heating rate setting satisfies: P3 stage ≤ P4 stage ≤ P5 stage)
[0019] If P4>P1, the heating rate of the fifth stage is adjusted to reach P5≤P1, and it is judged that the cracking of AlN during the sintering process of WC-Co-Ni-Cr-Al material has been completed; if P5≤P1 cannot be achieved after adjustment, it is judged that the cracking of AlN is not completely completed, and pore defects may appear in the metallographic structure of the alloy material after sintering, which is a structural defect that is difficult to repair, and the alloy material can only be scrapped.
[0020] AlN cracking is determined by two factors: temperature and vacuum. The smaller the vacuum value, the lower the cracking temperature, and vice versa. The higher the temperature required for cracking. The solid-phase sintering temperature of cemented carbide generally does not exceed 1320℃~1350℃. AlN cracking is completed before the end of solid-phase sintering. The smaller the vacuum value, the more favorable it is to complete the cracking at a lower temperature. The change of vacuum degree in the solid phase stage is dynamic, and the vacuum degree can be adjusted by the heating rate. However, when the escape rate of volatiles in the material exceeds the vacuum limit capacity of the sintering equipment, the vacuum value of the P3 section is very high, AlN stops cracking, and the vacuum system is still working. The residual AlN will continue to crack after the vacuum degree and temperature meet the conditions, and P4≥P1 will occur.
[0021] When designing the solid-phase sintering process, the heating rates of P3 to P5 should be designed based on the actual vacuum capacity P1 of the sintering equipment, with priority given to completing the vacuum cracking process of AlN in P4. P5 is the finishing stage, taking into account both the production cycle and cost control.
[0022] Generally, the sintering process of cemented carbide is roughly divided into three stages, namely, forming agent removal, solid phase sintering, and liquid phase sintering. After the forming agent removal stage is generally completed at 500℃~600℃, the solid phase sintering heating stage is entered, and the temperature is raised to 1320℃~1350℃ to complete the solid phase sintering, followed by the high temperature stage for liquid phase sintering, and finally cooling. In WC-Co-Ni-Cr-Al materials, since Al is added in the form of AlN, the AlN cracking during the sintering process is mainly completed in the solid phase stage, which is also the key step to complete the densification sintering of the alloy material, that is, the control of AlN cracking during the sintering process. If the residual AlN that has not been cracked enters the liquid phase sintering stage, it may cause bubble pores and Al oxide precipitation, affecting the density of the alloy structure. Since AlN vacuum cracking is possible only under vacuum heating conditions, relevant papers have reported that AlN can be cracked at above 800°C under vacuum conditions. Therefore, the present invention designs the solid phase sintering stages of WC-Co-Ni-Cr-Al products: the first stage is a heat preservation section at 700°C to 800°C, the second stage is a temperature increase of 800°C to 1000°C, the third stage is 1000°C to 1250°C, the fourth stage is a verification stage of 1250°C to 1290°C, and the fifth stage is a finishing stage of 1290°C to 1320°C.
[0023] The heating rate ΔT (0.2℃ / min~2.5℃ / min) and vacuum values P1~P5 (1.0Pa~20Pa) of the five different stages of solid phase sintering of WC-Co-Ni-Cr-Al material are designed and monitored to determine whether the cracking of AlN in WC-Co-Ni-Cr-Al material is completed and to ensure that the alloy material enters liquid phase sintering after the solid phase sintering is completed.
[0024] Preferably, the fsss particle size of the coarse WC powder is ≥20 μm.
[0025] Preferably, in the wet grinding mixing, the grinding medium is hexane, and the ball-to-material ratio is (2.5-2.0):1.
[0026] Preferably, the insulation time of the insulation section is ≥30 min.
[0027] Preferably, the heating rate of the second stage to the fifth stage is 0.2°C / min to 2.5°C / min.
[0028] Preferably, the liquid phase sintering is performed at a temperature of 1400° C. to 1460° C. for 1 hour.
[0029] Preferably, the vacuum heat treatment is a heat preservation treatment at 600° C. to 650° C. for 28 h to 32 h.
[0030] It can be seen from the above technical solution that compared with the prior art, the present invention has the following beneficial effects:
[0031] 1. The densification problem of WC-Co-Ni-Cr-Al large products is solved by combining vacuum degree with heating rate. The metallographic porosity of large products prepared by this method is not less than A02B00.
[0032] 2. Using the changing trend of the vacuum value, observation and control are performed at different stages of solid-phase sintering to accurately determine whether the cracking of AlN during the sintering process is completed.
[0033] 3. Utilize the common sintering equipment in the existing cemented carbide industry, adopt the design of the vacuum value change trend and heating rate in the furnace to control the cracking of AlN, and complete the densification sintering of WC-Co-Ni-Cr-Al materials, without the investment of additional new equipment, which is convenient for mass production. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0035] Figure 1 Schematic diagram of general cemented carbide sintering process.
[0036] Figure 2 This is a schematic diagram of the sintering process of WC-Co-Ni-Cr-AlN material implemented in the present invention.
[0037] Figure 3 This is a low-magnification metallographic image of Example 1 WC-32% (Co+Ni)-1.0% Cr-2.7% AlN.
[0038] Figure 4 This is a low-magnification metallographic image of comparative example 1 WC-32% (Co+Ni)-1.0% Cr-2.7% AlN.
[0039] Figure 5 This is a low-magnification metallographic image of Example 2 WC-24% (Co+Ni)-0.8% Cr-1.8% AlN.
[0040] Figure 6 This is a low-magnification metallographic image of the comparative example 2WC-24% (Co+Ni)-0.8% Cr-1.8% AlN.
[0041] Figure 7 This is a low-magnification metallographic image of Example 3 WC-15% (Co+Ni)-0.5% Cr-0.8% AlN.
[0042] Figure 8This is a low-magnification metallographic image of the comparative example 3WC-15% (Co+Ni)-0.5% Cr-0.8% AlN. DETAILED DESCRIPTION
[0043] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0044] The present invention adopts a powder metallurgy method, and takes the sintering of a block product with a single weight of 40-45kg and a diameter of φ200mm made of a hard alloy material with a Co-Ni content of 15-32% as an example for explanation. In the general sintering process for WC-Co-Ni-Cr-AlN powder material, insufficient cracking of AlN will cause Al oxide precipitation in the alloy microstructure, resulting in alloy defects. For alloy materials with different compositions, the process of the solid phase heating sintering stage is designed.
[0045] Figure 1 This is a schematic diagram of the general cemented carbide sintering process. The solid phase sintering temperature rises from 700℃ to 1320℃, the sintering furnace is in a negative pressure state, and the heating rate is 2.5℃ to 5.0℃ / min. The comparative heating rate is 3.5℃ / min for the test;
[0046] Figure 2 This is a schematic diagram of the sintering process of WC-Co-Ni-Cr-AlN material implemented in the present invention.
[0047] The solid phase sintering temperature rise in the 700℃~1320℃ stage is designed in stages. The vacuum degree in the sintering furnace is in a negative pressure state. At the same time, the vacuum degree and the heating rate are monitored and controlled. The design is carried out according to Table 1, and different parameters are selected according to the alloy material composition, product weight and volume size.
[0048] Table 1 Temperature rise and vacuum control scheme of 700℃~1320℃ in solid phase sintering stage
[0049]
[0050] The maximum vacuum value in the P4 stage is used as the basis for judgment, and the following situations are judged:
[0051] 1) When P4≤P1, P4<P3, P5<P4 are satisfied at the same time, it can be judged that the cracking of AlN during the sintering process of WC-Co-Ni-Cr-Al material has been completed.
[0052] 2) When P4 ≥ (1-2) times P1 or above, if P5 ≤ P1 is reached by adjusting the heating rate, it can also be judged that the cracking of AlN during the sintering process of WC-Co-Ni-Cr-Al material has been completed; if P5 ≤ P1 is not reached, the cracking of AlN is not completed.
[0053] Example 1
[0054] Take 64.3 parts of WC powder with a Fisher particle size of 20.0μm, 16 parts of Co powder and mix them with 16 parts of Ni powder, 1 part of Cr powder and 2.7 parts of AlN powder. For every kilogram of mixed powder, the amount of hexane added is 0.30L, the amount of paraffin added is 0.2g, and the amount of solvent added is 0.02g. Mix WC powder, Co powder, paraffin, solvent, etc. and load them into a ball mill with a ball-to-material ratio of 2.5:1 and a ball milling time of 28h. After unloading, drying, granulation and pressing, a green compact is obtained with a green compact weight of 40.5kg; then solid-phase sintering is carried out using the scheme in Table 2. After the solid-phase sintering is completed, the alloy is sintered at 1400℃ for 1h to obtain a grain size of 2.43um and a porosity of A02B00. After sintering, vacuum heat treatment is carried out at a temperature of 620℃ for 32h. The metallographic structure is as follows Figure 3 As shown in Table 2, no pores caused by Al oxides were found. The control of vacuum degree and heating rate during solid phase sintering is shown in Table 2.
[0055] Table 2 Vacuum degree and heating rate control
[0056]
[0057] Comparative Example 1
[0058] The composition is the same as that of Example 1. Under the same conditions, wet grinding, mixing, drying and granulation are carried out, and the green body is pressed and then sintered. Except for the process scheme of the solid phase sintering stage, the other processes are the same. The solid phase sintering stage is 700℃~1320℃ with a heating rate of 3.5℃ / min, and the vacuum degree in the sintering furnace is in a negative pressure state. Figure 4 The properties of the alloys of Example 1 and Comparative Example 1 are shown in Table 3.
[0059] Table 3 Basic properties of alloys in Example 1 and Comparative Example 1
[0060]
[0061]
[0062] Example 2
[0063] Take 73.4 parts of WC powder with a Fisher particle size of 20.0μm, 12 parts of Co powder and mix them with 12 parts of Ni powder, 0.8 parts of Cr powder and 1.8 parts of AlN powder. For every kilogram of mixed powder, the amount of hexane added is 0.30L, the amount of paraffin added is 0.2g, and the amount of solvent added is 0.02g. Mix WC powder, Co powder, paraffin, solvent, etc. and load them into a ball mill with a ball-to-material ratio of 2.5:1 and a ball milling time of 28h. After unloading, drying, granulation and pressing, a green compact is obtained with a green compact weight of 43kg; then solid-phase sintering is carried out using the scheme in Table 4. After solid-phase sintering, the alloy is sintered at 1410℃ for 1h to obtain an alloy with a grain size of 2.39μm and a porosity of A02B00. After sintering, vacuum heat treatment is carried out at a temperature of 650℃ for 28h. The metallographic structure is as follows Figure 5 As shown in Table 4, no pores caused by Al oxides were found. The control of vacuum degree and heating rate during the solid phase sintering stage is shown in Table 4.
[0064] Table 4 Vacuum degree and heating rate control
[0065]
[0066] Comparative Example 2
[0067] The composition is the same as that of Example 2. Under the same conditions, wet grinding, mixing, drying and granulation are carried out, and the green body is pressed and then sintered. The sintering process is the same except that the process scheme of the solid phase sintering stage is different. The solid phase sintering stage is 700℃~1320℃ with a heating rate of 3.5℃ / min, and the vacuum degree in the sintering furnace is in a negative pressure state. Figure 6 The metallographic pores are A02B04. The partial properties of the alloys of Example 2 and Comparative Example 2 are shown in Table 5.
[0068] Table 5 Basic properties of alloys in Example 2 and Comparative Example 2
[0069]
[0070] Example 3
[0071] Take 83.7 parts of WC powder with a Fisher particle size of 20.0μm, 7.5 parts of Co powder and mix them with 7.5 parts of Ni powder, 0.5 parts of Cr powder and 0.8 parts of AlN powder. For every kilogram of mixed powder, the amount of hexane added is 0.30L, the amount of paraffin added is 0.2g, and the amount of solvent added is 0.02g. The WC powder, Co powder, paraffin, solvent, etc. are mixed and loaded into a ball mill with a ball-to-material ratio of 2.0:1 and a ball milling time of 28h. After unloading, drying, granulation and pressing, a green compact is obtained with a green compact weight of 42.0kg; then solid-phase sintering is carried out using the scheme in Table 6. After the solid-phase sintering is completed, the alloy is sintered at 1460℃ for 1h to obtain a grain size of 2.14μm and a porosity of A02B00. After sintering, vacuum heat treatment is carried out at a temperature of 630℃ for 30h. The metallographic structure is as follows Figure 7 As shown in Table 6, no pores caused by Al oxides were found. The control of vacuum degree and heating rate during the solid phase sintering stage is shown in Table 6.
[0072] Table 6 Vacuum degree and heating rate control
[0073]
[0074]
[0075] Comparative Example 3
[0076] The composition is the same as that of Example 3. Under the same conditions, wet grinding, mixing, drying and granulation are carried out, and the green body is pressed and then sintered. Except for the process scheme of the solid phase sintering stage, the other processes are the same. The solid phase sintering stage is 700℃~1320℃ with a heating rate of 3.5℃ / min, and the vacuum degree in the sintering furnace is in a negative pressure state. Figure 8 The properties of the alloys of Example 3 and Comparative Example 3 are shown in Table 7.
[0077] Table 7 Basic properties of alloys in Example 3 and Comparative Example 3
[0078]
[0079] By comparing the metallographic structures and mechanical properties of the embodiments and comparative examples, it is found that after the implementation of this technical solution, the density of the sintered body of the WC-Co-Ni-Cr-Al material is improved, and the strength and hardness of the alloy are greatly improved through subsequent vacuum heat treatment. In particular, the improvement of the alloy strength is the most obvious. The solution to the densification problem of the WC-Co-Ni-Cr-Al material in the sintering stage plays a positive role in improving the performance of the subsequent alloy after heat treatment.
[0080] In this specification, each embodiment is described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the embodiments can be referred to each other. For the device disclosed in the embodiment, since it corresponds to the method disclosed in the embodiment, the description is relatively simple, and the relevant parts can be referred to the method part.
[0081] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A cemented carbide containing WC, Co, Ni, Cr and Al, characterized in that: In terms of mass percentage, it includes the following components: Co7.5-16%, Ni7.5-16%, Cr0.5-1.0%, AlN0.8-2.7%, and the balance is WC; Among them, the mass ratio of Co to Ni is 1:
1.
2. A cemented carbide containing WC, Co, Ni, Cr and Al as claimed in claim 1, characterized in that: The particle size of the AlN powder is ≤2 μm.
3. The method for preparing a cemented carbide containing WC, Co, Ni, Cr and Al as claimed in claim 1, characterized in that: include: AlN powder is wet-milled and mixed with coarse WC powder, Co powder, Ni powder, Cr powder / Cr carbide, and then dried, sieved, granulated, pressed into green embryos in sequence after ball milling to a certain point, and then the forming agent is removed, solid phase sintering, liquid phase sintering and vacuum heat treatment are carried out in sequence; The solid phase sintering includes: a first stage of setting a heat preservation section at 700°C to 800°C, during which the vacuum is reduced to a limit of ≤5Pa; a second stage of heating at (700-800)°C to 1000°C; a third stage of heating at 1000°C to 1250°C; a fourth stage of heating at 1250°C to 1290°C; and a fifth stage of heating at 1290°C to 1320°C; The vacuum degree in the five solid-phase sintering stages was monitored and named P1, P2, P3, P4 and P5, respectively, where P1 took the minimum value and P2-P5 took the maximum value; The minimum value of P1 is used as the basis for comparison. When P4≤P1, P4<P3, and P5<P4 are satisfied at the same time, it is judged that the cracking of AlN during the sintering process of WC-Co-Ni-Cr-Al material has been completed, and liquid phase sintering is directly entered; If P4>P1, the heating rate of the fifth stage is adjusted to reach P5≤P1, and it is judged that the cracking of AlN during the sintering process of WC-Co-Ni-Cr-Al material has been completed; if P5≤P1 cannot be achieved after adjustment, it is judged that the cracking of AlN has not been completely completed, and the alloy material is scrapped.
4. The method for preparing a cemented carbide containing WC, Co, Ni, Cr and Al components according to claim 3, characterized in that: The fsss particle size of the coarse WC powder is ≥20 μm.
5. The method for preparing a cemented carbide containing WC, Co, Ni, Cr and Al components according to claim 3, characterized in that: In the wet grinding mixing, the grinding medium is hexane, and the ball-to-material ratio is (2.5-2.0):
1.
6. The method for preparing a cemented carbide containing WC, Co, Ni, Cr and Al as claimed in claim 3, characterized in that: The insulation time of the insulation section is ≥30min.
7. The method for preparing a cemented carbide containing WC, Co, Ni, Cr and Al as claimed in claim 3, characterized in that: The heating rate of the second stage to the fifth stage is 0.2°C / min to 2.5°C / min.
8. The method for preparing a cemented carbide containing WC, Co, Ni, Cr and Al as claimed in claim 3, characterized in that: The liquid phase sintering is carried out by heat preservation treatment at 1400° C. to 1460° C. for 1 hour.
9. The method for preparing a cemented carbide containing WC, Co, Ni, Cr and Al as claimed in claim 3, wherein the vacuum heat treatment is a heat preservation treatment at 600°C to 650°C for 28h to 32h.
Citation Information
Patent Citations
Twin-crystal WC structure cemented carbide and preparation method thereof
CN111088449A
YA type gradient hard alloy material with hard surface and tough interior
CN113621859A
Matrix material of Al-containing hard alloy numerical control blade and preparation method of matrix material
CN117778850A
Tungsten carbide-base hard alloy for hot-working apparatus members
EP0062311A1
Ceramic crystal grain, ceramic sintered compact and method for producing them
JP2014185054A
Cited By
Cutting tool
EP4756053A1
Cutting tool
WO2026120125A1