Production method of ferromanganese
By utilizing the sensible heat of liquid slag to react with manganese silicon alloy powder and ferrosilicon powder during the production of ferromanganese, the problems of high consumption and high cost of manganese silicon alloy in the production of ferromanganese have been solved, and the efficient production and cost reduction of ferromanganese alloy have been achieved.
Patent Information
- Application Number
- CN202411383741.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-11-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the existing electrosilicon thermal process for ferromanganese production, the heat of the high-temperature liquid slag is not effectively utilized, the manganese recovery rate in the slag is low, and the consumption of ferromanganese alloy is large, resulting in high costs and increased workload.
During the smelting process, the sensible heat of the liquid slag is used to react with manganese silicon alloy powder and ferrosilicon powder to extract effective elements from the slag, reduce the production of manganese-rich slag, and carry out alloying reaction in the ladle to increase the manganese content of the molten iron and reduce the consumption of manganese silicon alloy powder.
By effectively utilizing the sensible heat of liquid slag, the consumption of manganese silicon alloy powder was reduced, the smelting time was shortened, the power consumption was reduced, the yield and quality of manganese ferroalloys were improved, and the production cost was reduced.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ferromanganese alloy production, in particular to a method for producing ferromanganese. Background Art
[0002] The electro-silicon thermal method is a common method for producing ferromanganese. Specifically, the electro-silicon thermal method for smelting ferromanganese is to add manganese ore raw materials, manganese-silicon alloy (reducing agent) and lime into a refining electric furnace or a shaking bag, mainly relying on electric heat to melt the charge, and refine and desiliconize the silicon-manganese alloy to obtain ferromanganese, and then discharge the upper slag water, and pour and cool the lower molten iron to obtain ferromanganese alloy. However, the temperature of the discharged slag water is relatively high, and the manganese content of the slag is 16% to 24%, which is a high-temperature liquid rich slag. At present, the common slag treatment method is to directly cool the aforementioned high-temperature liquid rich slag into slag, and the heat in the cooling process cannot be effectively utilized; after the slag is cooled, it is crushed into qualified particle size raw materials for the production of manganese-silicon alloy. The manganese content of the slag in the production process of manganese-silicon alloy is about 8%, and the manganese recovery rate in the slag is limited. After the slag solidifies, the entire process needs to be transported and crushed at the same time, which not only increases the workload, but also increases the cost. In addition, in the production of ferromanganese alloy, a large amount of manganese-silicon alloy still needs to be invested, and there are problems of large consumption and high cost of manganese-silicon alloy. Summary of the invention
[0003] The object of the present invention is to provide a method for producing ferromanganese.
[0004] The present invention is implemented by the following technical scheme: a method for producing ferromanganese, comprising the following steps: S1 Preheating Smelting Furnace Power on the electrodes of the smelting furnace to preheat the smelting furnace, control the current of the electrodes to 50-100A, and preheat for 20-30 minutes; S2 furnace start Putting manganese ore raw materials, lime and manganese-silicon alloy powder into a preheated smelting furnace for smelting, and then performing slag separation, pouring the separated molten iron into a casting pool for casting and molding to obtain a first manganese-ferroalloy product, and pouring the separated liquid slag into a shaking bag; S3 Shake Bag Adding manganese-silicon alloy powder and ferrosilicon powder into the shake bag, and rotating the shake bag to make the manganese-silicon alloy powder and ferrosilicon powder melt and react; S4 Shake-up bag separation After S3 is completed, the shaking bag is tilted, and the liquid slag and liquid alloy in the shaking bag are poured into the molten iron ladle together. The molten iron ladle is left to stand for 1-10 minutes to allow the slag in the molten iron ladle to float up, and then the floating slag is poured out and cooled to obtain lean slag; S5 Smelting After S4 is finished, the slag in the ladle is dumped out, and the remaining molten iron in the ladle is sent to the smelting furnace, and manganese ore raw materials, lime and manganese silicon alloy powder are added to the smelting furnace for smelting; S6 smelting and slag separation After S5 is finished, the furnace is opened and the molten iron and liquid slag in the smelting furnace are poured into a ladle for slag separation. The separated molten iron is poured into a casting pool for casting and molding to obtain a second ferromanganese alloy product. The separated liquid slag is poured into a shaking ladle, and the above steps S3 to S5 are repeated; S7 Final Slag Treatment After S6 is completed, the separated liquid slag is subjected to final slag treatment to obtain final slag.
[0005] Furthermore, the S2 specifically includes the following steps: S2-1: putting manganese ore raw material, lime and manganese silicon alloy powder into a smelting furnace according to the weight ratio of 100:45-65:55-60 for smelting; S2-2 After smelting, the furnace is opened and the molten iron and liquid slag are poured into the ladle for slag separation. The separated molten iron is poured into the casting pool for casting and molding, and the separated liquid slag is poured into the shaking ladle.
[0006] Furthermore, in S2-1, the electrode current of the smelting furnace is controlled to be 380-440A, the furnace temperature is controlled to be 1800-2000°C, and the smelting time is 130-160min.
[0007] Furthermore, in S3, the weight ratio of liquid slag, manganese silicon alloy powder and ferrosilicon powder is 15:(1-2):(1-2).
[0008] Furthermore, in S3, when adding manganese silicon alloy powder and ferrosilicon powder to the shaking bag, the rotation speed of the shaking bag is controlled to be 500-700 r / min and the feeding rate is controlled to be 0.5-1 t / min; during the melting process, the rotation speed of the shaking bag is controlled to be 700-1000 r / min and the shaking time is 6-12 min.
[0009] Furthermore, in S3, the ferrosilicon powder contains Si≥65%, C 0.05%-0.7%, and P 0.02%-0.10% by weight; the manganese silicon alloy powder contains Mn 58%-64%, Si 24%-32%, C 0.05%-0.4%, and P 0.07%-0.12% by weight.
[0010] Furthermore, in S5, the manganese ore raw material, lime, molten iron, and manganese silicon alloy powder are mixed in a weight ratio of 100:40-60:20-45:40-50.
[0011] Furthermore, in S5, during the smelting process, the electrode current is controlled to be 350-420A, the furnace temperature is controlled to be 1800-2000°C, and the smelting is performed for 110-135 minutes.
[0012] Furthermore, in S2 and S6, the liquid slag is controlled to contain 16% to 24% Mn, 30% to 40% CaO and SiO in weight percentage. 2 25% to 32%; the slag basicity CaO / SiO of the liquid rich slag 2 It is 1.15~1.4.
[0013] Furthermore, the S7 final slag treatment is to cool the liquid slag separated from S6 to obtain manganese-rich slag, or to repeat the treatment process from S3 to S4 for the liquid slag separated from S6, and finally cast the remaining molten iron in the ladle into ingots to obtain a manganese-iron alloy reducing agent.
[0014] The advantages of the present invention are as follows: the present invention only needs to input a large proportion of manganese silicon alloy powder in the furnace startup stage. After the furnace startup is completed, the liquid slag separated from the refining furnace can be sent to the shaking bag, and the sensible heat of the liquid slag is used to react with the added manganese silicon alloy powder and ferrosilicon powder to extract the effective elements in the liquid slag, so that the slag is enriched and the output of manganese-rich slag is reduced. The manganese content of the molten iron after the shaking bag is relatively high, and part of the manganese silicon alloy powder can be directly put into the smelting furnace as a reducing agent, thereby reducing the consumption of manganese silicon alloy powder and reducing the cost investment; and the temperature of the molten iron after the shaking bag is relatively high, and it can be directly put into the smelting furnace, which is helpful to shorten the smelting time and reduce the power consumption. DETAILED DESCRIPTION
[0015] Embodiment 1: A method for producing ferromanganese, comprising the following steps: S1 Preheating Smelting Furnace The electrodes of the smelting furnace are powered on to preheat the smelting furnace. The current of the electrodes is controlled to be 50A and the preheating time is 20 minutes.
[0016] S2 furnace start Putting manganese ore raw materials, lime and manganese-silicon alloy powder into a preheated smelting furnace for smelting, and then performing slag separation, pouring the separated molten iron into a casting pool for casting and molding to obtain a first manganese-ferroalloy product, and pouring the separated liquid slag into a shaking bag; S2 specifically includes the following steps: S2-1 puts 15t manganese ore raw materials, 6.75t lime and 8.25t manganese silicon alloy powder into the smelting furnace for smelting; controls the smelting furnace electrode current to 380A, controls the furnace temperature to 2000℃, and smelts for 130min.
[0017] After S2-2 smelting is completed, the furnace is opened and the molten iron and liquid slag are poured into a ladle for slag separation. The separated molten iron is poured into a casting pool for casting and molding to obtain 8.83t of the first ferrosilicon alloy product, and the separated 15t of liquid slag is poured into a shaking ladle.
[0018] S3 Shake Bag Add 2t of manganese-silicon alloy powder and 2t of ferrosilicon powder to the shaking bag. When adding manganese-silicon alloy powder and ferrosilicon powder to the shaking bag, the rotation speed of the shaking bag is controlled to be 700r / min and the feeding speed is controlled to be 0.5t / min; wherein, the ferrosilicon powder contains Si65%, C 0.05% and P 0.02% by weight; the manganese-silicon alloy powder contains Mn 64%, Si 24%, C 0.4% and P 0.12% by weight.
[0019] The shaking bag was rotated to make the manganese silicon alloy powder and ferrosilicon powder melt and react. During the melting process, the shaking bag speed was controlled at 1000r / min and the shaking time was 12min. S4 Shake-up bag separation After S3 is completed, the shaking bag is tilted, and the liquid slag and liquid alloy in the shaking bag are poured into the molten iron ladle together. The molten iron ladle is left to stand for 10 minutes to allow the slag in the molten iron ladle to float up, and then the floating slag is poured out and cooled to obtain lean slag; S5 Smelting After S4 is completed, the remaining 6.8t of molten iron in the ladle is sent to the smelting furnace, and 15t of manganese ore raw material, 6t of lime and 6t of manganese silicon alloy powder are added to the smelting furnace for smelting. During the smelting process, the electrode current is controlled at 350A, the furnace temperature is controlled at 1800℃, and the smelting time is 110min.
[0020] S6 smelting and slag separation After S5 is completed, the furnace is opened and the molten iron and liquid slag in the smelting furnace are poured into a ladle for slag separation. The separated molten iron is poured into a casting pool for casting and molding to obtain a second manganese-iron alloy product. The separated 15t liquid slag is poured into a shaking ladle, and the above steps S3 to S5 are repeated.
[0021] In S2 and S6, the liquid slag is controlled to contain 24% Mn, 30% CaO and 30% SiO by weight. 2 25%; Liquid rich slag slag basicity CaO / SiO 2 is 1.2.
[0022] S7 Final Slag Treatment After S6 is completed, the liquid slag separated from S6 is cooled to obtain 15t of manganese-rich slag.
[0023] Embodiment 2: A method for producing ferromanganese, comprising the following steps: S1 Preheating Smelting Furnace The electrodes of the smelting furnace are energized to preheat the smelting furnace, the current of the electrodes is controlled to be 100A, and the preheating time is 30 minutes.
[0024] S2 furnace start Putting manganese ore raw materials, lime and manganese-silicon alloy powder into a preheated smelting furnace for smelting, and then performing slag separation, pouring the separated molten iron into a casting pool for casting and molding to obtain a first manganese-ferroalloy product, and pouring the separated liquid slag into a shaking bag; S2 specifically includes the following steps: S2-1 puts 15t manganese ore raw materials, 9.75t lime and 9t manganese silicon alloy powder into the smelting furnace for smelting; controls the smelting furnace electrode current to 440A, controls the furnace temperature to 1800℃, and smelts for 160min.
[0025] After S2-2 smelting is completed, the furnace is opened and the molten iron and liquid slag are poured into a ladle for slag separation. The separated molten iron is poured into a casting pool for casting and molding to obtain 10.04t of the first ferrosilicon alloy product, and the separated 15t of liquid slag is poured into a shaking ladle.
[0026] S3 Shake Bag Add 1 t of manganese silicon alloy powder and 1 t of ferrosilicon powder into the shaking bag. When adding the manganese silicon alloy powder and ferrosilicon powder into the shaking bag, the rotation speed of the shaking bag is controlled to be 500r / min and the feeding speed is controlled to be 1 t / min. Among them, the ferrosilicon powder contains Si 70%, C 0.7% and P 0.10% by weight; the manganese silicon alloy powder contains Mn 58%, Si 32%, C 0.05% and P 0.07% by weight.
[0027] The shaking bag was rotated to make the manganese silicon alloy powder and ferrosilicon powder melt and react. During the melting process, the shaking bag speed was controlled at 700r / min and the shaking time was 6min. S4 Shake-up bag separation After S3 is completed, the shaking bag is tilted, and the liquid slag and liquid alloy in the shaking bag are poured into the molten iron ladle together. The molten iron ladle is left to stand for 1 minute to allow the slag in the molten iron ladle to float up, and then the floating slag is poured out and cooled to obtain lean slag; S5 Smelting After S4 is completed, the remaining 3.4t of molten iron in the ladle is sent to the smelting furnace, and 15t of manganese ore raw materials, 9t of lime and 7.5t of manganese silicon alloy powder are added to the smelting furnace for smelting. During the smelting process, the electrode current is controlled at 420A, the furnace temperature is controlled at 2000℃, and the smelting time is 135min.
[0028] S6 smelting and slag separation After S5 is completed, the furnace is opened and the molten iron and liquid slag in the smelting furnace are poured into a ladle for slag separation. The separated molten iron is poured into a casting pool for casting and molding to obtain a second manganese-iron alloy product. The separated 15t liquid slag is poured into a shaking ladle, and the above steps S3 to S5 are repeated.
[0029] In S2 and S6, the liquid slag is controlled to contain 16% Mn, 40% CaO and 40% SiO by weight. 2 28.6%; Liquid rich slag slag basicity CaO / SiO 2 is 1.4.
[0030] S7 Final Slag Treatment After S6 is completed, the liquid slag separated from S6 is cooled to obtain 15t of manganese-rich slag.
[0031] Embodiment 3: A method for producing ferromanganese, comprising the following steps: S1 Preheating Smelting Furnace The electrodes of the smelting furnace are powered on to preheat the smelting furnace. The current of the electrodes is controlled to be 70A and the preheating time is 25 minutes.
[0032] S2 furnace start Putting manganese ore raw materials, lime and manganese-silicon alloy powder into a preheated smelting furnace for smelting, and then performing slag separation, pouring the separated molten iron into a casting pool for casting and molding to obtain a first manganese-ferroalloy product, and pouring the separated liquid slag into a shaking bag; S2 specifically includes the following steps: S2-1 puts 15t manganese ore raw material, 8.3t lime and 8.7t manganese silicon alloy powder into the smelting furnace for smelting; controls the smelting furnace electrode current to 400A, controls the furnace temperature to 1900℃, and smelts for 140min.
[0033] After S2-2 smelting is completed, the furnace is opened and the molten iron and liquid slag are poured into a ladle for slag separation. The separated molten iron is poured into a casting pool for casting and molding to obtain 9.24t of the first ferrosilicon alloy product, and the separated 15t of liquid slag is poured into a shaking ladle.
[0034] S3 Shake Bag 1.5t of manganese silicon alloy powder and 1.5t of ferrosilicon powder are added to the shaking bag. When adding the manganese silicon alloy powder and ferrosilicon powder to the shaking bag, the rotation speed of the shaking bag is controlled to be 600r / min and the feeding speed is controlled to be 0.7t / min; wherein, the ferrosilicon powder contains Si65%, C 0.2% and P 0.08% by weight; the manganese silicon alloy powder contains Mn 60%, Si 26.5%, C 0.25% and P 0.09% by weight.
[0035] The shaking bag was rotated to make the manganese silicon alloy powder and the ferrosilicon powder melt and react. During the melting process, the shaking bag speed was controlled to be 900r / min and the shaking time was 10min. S4 Shake-up bag separation After S3 is completed, the shaking bag is tilted, and the liquid slag and liquid alloy in the shaking bag are poured into the molten iron ladle together. The molten iron ladle is left to stand for 6 minutes to allow the slag in the molten iron ladle to float up, and then the floating slag is poured out and cooled to obtain lean slag; S5 Smelting After S4 is completed, the remaining 5.1t of molten iron in the ladle is sent to the smelting furnace, and 15t of manganese ore raw material, 8.3t of lime and 6.33t of manganese silicon alloy powder are added into the smelting furnace for smelting. During the smelting process, the electrode current is controlled at 400A, the furnace temperature is controlled at 1900℃, and the smelting is carried out for 120min.
[0036] S6 smelting and slag separation After S5 is completed, the furnace is opened and the molten iron and liquid slag in the smelting furnace are poured into a ladle for slag separation. The separated molten iron is poured into a casting pool for casting and molding to obtain a second manganese-iron alloy product. The separated 15t liquid slag is poured into a shaking ladle, and the above steps S3 to S5 are repeated.
[0037] In S2 and S6, the liquid slag is controlled to contain 19% Mn, 36.8% CaO and 1.5% SiO2 by weight. 2 32%; Liquid rich slag slag basicity CaO / SiO 2 is 1.15.
[0038] S7 Final Slag Treatment After S6 is completed, the liquid slag separated from S6 is cooled to obtain 15t of manganese-rich slag.
[0039] Comparative Example: A method for producing ferromanganese, comprising the following steps: S1 Preheating Smelting Furnace Power on the electrodes of the smelting furnace to preheat the smelting furnace, control the current of the electrodes to 50-100A, and preheat for 20-30 minutes; S2 Smelting Put 30t manganese ore raw material, 19.2t lime and 17.98t manganese silicon alloy powder into the smelting furnace, control the electrode current to 420A, control the furnace temperature to 2000℃, and smelt for 150min; S3 Slag separation After smelting, the furnace is opened and the molten iron and liquid slag are poured into the ladle for slag separation. The separated molten iron is poured into the casting pool for casting and molding to obtain 19.25t of manganese-ferroalloy products. The separated liquid slag is cooled to obtain 30t of manganese-rich slag. Take 30t of manganese ore raw material (the same batch of manganese ore raw material as that treated in the comparative example) as an example, wherein 15t of manganese ore raw material is used in the start-up process of S2, and the remaining 15t of manganese ore raw material is treated by the smelting process of S5, and the second alloy products of 12.85t, 10.90t and 12.43t are obtained respectively. The raw material consumption, the output and purity of the ferromanganese alloy products are statistically analyzed as shown in the following table:
[0040] At present, the market price of ferrosilicon powder is 5707 yuan / ton, the market price of manganese silicon alloy powder is 5735 yuan / ton, the market price of lime is 424 yuan / ton, the market price of manganese ore raw material is 1610 yuan / ton, the market price of manganese-rich slag is 530 yuan / ton, the electricity fee is 0.40 yuan / kwh, and the ferromanganese alloy product is 8053 yuan / ton. The cost of Example 1 is 157734.95 yuan, and the income is 16854.09 yuan; the cost of Example 2 is 161489.10 yuan, and the income is 7140.72 yuan; the cost of Example 3 is 158116.45 yuan, and the income is 16392.06 yuan; the cost of the comparative example is 152896.10 yuan, and the income is 2124.15 yuan. In comprehensive comparison, the ferromanganese production method adopted in the present invention can reduce power consumption, reduce the consumption of manganese silicon alloy powder, increase the output of ferromanganese alloy and the manganese content of the product, thereby achieving the purpose of energy saving, improving profits and product quality.
[0041] Example 4: A method for producing ferromanganese, the treatment process of which is the same as that of Example 1, except that the S7 final slag treatment is to repeat the treatment process from S3 to S4 on the liquid slag separated from S6, and finally the remaining molten iron in the ladle is cast into ingots to finally obtain 6.8t of ferromanganese alloy reducing agent.
[0042] Example 5: A method for producing ferromanganese, the treatment process of which is the same as that of Example 2, except that the S7 final slag treatment is to repeat the treatment process from S3 to S4 on the liquid slag separated from S6, and finally the remaining molten iron in the ladle is cast into ingots to finally obtain 3.4t of ferromanganese alloy reducing agent.
[0043] Example 6: A method for producing ferromanganese, the treatment process of which is the same as that of Example 3, except that the S7 final slag treatment is to repeat the treatment process from S3 to S4 for the liquid slag separated from S6, and finally the remaining molten iron in the ladle is cast into ingots to finally obtain 5.1t of ferromanganese alloy reducing agent.
[0044] The main component contents of the ferromanganese alloy reducing agents obtained in Examples 4 to 6 were tested, and the test results are shown in the following table:
[0045] It can be seen from the above table that the manganese content of the ferromanganese alloy reducing agent obtained in Examples 1 to 3 is above 74%, the silicon content is below 12.5%, and the phosphorus content is 0.08% or below. It has the characteristics of high manganese, low silicon and low phosphorus, and can be used as a reducing agent for producing ferromanganese alloy; and the manganese content of the lean slag obtained by S4 shaking ladle slag separation is below 8%, achieving the depletion of rich slag.
[0046] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for producing ferromanganese, characterized in that: It includes the following steps: S1 Preheating Smelting Furnace Power on the electrodes of the smelting furnace to preheat the smelting furnace, control the current of the electrodes to 50-100A, and preheat for 20-30 minutes; S2 furnace start Putting manganese ore raw materials, lime and manganese-silicon alloy powder into a preheated smelting furnace for smelting, and then performing slag separation, pouring the separated molten iron into a casting pool for casting and molding to obtain a first manganese-ferroalloy product, and pouring the separated liquid slag into a shaking bag; S3 Shake Bag Adding manganese-silicon alloy powder and ferrosilicon powder into the shake bag, and rotating the shake bag to make the manganese-silicon alloy powder and ferrosilicon powder melt and react; S4 Shake-up bag separation After S3 is completed, the shaking bag is tilted, and the liquid slag and liquid alloy in the shaking bag are poured into the molten iron ladle together. The molten iron ladle is left to stand for 1-10 minutes to allow the slag in the molten iron ladle to float up, and then the floating slag is poured out and cooled to obtain lean slag; S5 Smelting After S4 is finished, the remaining molten iron in the ladle is sent to the smelting furnace, and manganese ore raw materials, lime and manganese silicon alloy powder are added to the smelting furnace for smelting; S6 smelting and slag separation After S5 is finished, the furnace is opened and the molten iron and liquid slag in the smelting furnace are poured into a ladle for slag separation. The separated molten iron is poured into a casting pool for casting and molding to obtain a second ferromanganese alloy product. The separated liquid slag is poured into a shaking ladle, and the above steps S3 to S5 are repeated; S7 Final Slag Treatment After S6 is completed, the separated liquid slag is subjected to final slag treatment to obtain final slag.
2. The method for producing ferromanganese according to claim 1, characterized in that: The S2 specifically includes the following steps: S2-1: putting manganese ore raw material, lime and manganese silicon alloy powder into a smelting furnace according to the weight ratio of 100:45-65:55-60 for smelting; S2-2 After smelting, the furnace is opened and the molten iron and liquid slag are poured into the ladle for slag separation. The separated molten iron is poured into the casting pool for casting and molding, and the separated liquid slag is poured into the shaking ladle.
3. The method for producing ferromanganese according to claim 2, characterized in that: In S2-1, the electrode current of the smelting furnace is controlled to be 380-440A, the furnace temperature is controlled to be 1800-2000°C, and the smelting is performed for 130-160 minutes.
4. The method for producing ferromanganese according to claim 1, characterized in that: In S3, the weight ratio of liquid slag, manganese silicon alloy powder and ferrosilicon powder is 15:(1-2):(1-2).
5. The method for producing ferromanganese according to claim 1, characterized in that: In S3, when adding manganese silicon alloy powder and ferrosilicon powder to the shaking bag, the rotation speed of the shaking bag is controlled to be 500-700r / min and the feeding speed is controlled to be 0.5-1t / min; during the melting process, the rotation speed of the shaking bag is controlled to be 700-1000r / min and the shaking time is 6-12min.
6. The method for producing ferromanganese according to claim 1, characterized in that: In the S3, the ferrosilicon powder contains Si≥65%, C 0.05%-0.7%, and P 0.02%-0.10% by weight; the manganese silicon alloy powder contains Mn 58%-64%, Si 24%-32%, C 0.05%-0.4%, and P 0.07%-0.12% by weight.
7. The method for producing ferromanganese according to claim 1, characterized in that: In S5, the manganese ore raw material, lime, molten iron, and manganese silicon alloy powder are mixed in a weight ratio of 100:40-60:20-45:40-50.
8. The method for producing ferromanganese according to claim 1, characterized in that: In S5, during the smelting process, the electrode current is controlled to be 350-420A, the furnace temperature is controlled to be 1800-2000°C, and the smelting is performed for 110-135 minutes.
9. The method for producing ferromanganese according to claim 1, characterized in that: In S2 and S6, the liquid slag is controlled to contain 16% to 24% Mn, 30% to 40% CaO and 25% to 32% SiO2 by weight; the slag basicity CaO / SiO2 of the liquid rich slag is 1.15 to 1.
4.
10. The method for producing ferromanganese according to claim 1, characterized in that: The S7 final slag treatment is to cool the liquid slag separated from S6 to obtain manganese-rich slag, or to repeat the treatment process from S3 to S4 for the liquid slag separated from S6, and finally cast the remaining molten iron in the ladle into ingots to obtain a manganese-iron alloy reducing agent.
Citation Information
Patent Citations
Production process for smelting medium-low carbon ferromanganese through manganese sesquicarbonate ores
CN106756350A
Method for preparing pure manganese iron alloy and active silicate particles by using inferior alloy powder
CN110669944A
Method for producing silicomanganese by using low-carbon ferromanganese
CN112941382A
Method for preparing low-carbon low-phosphor silicon manganese alloy by utilizing medium manganese slag and siliceous reducer
CN1837389A
Process for the production of ferromanganese products from managanese-bearing materials
GB827162A