Wide-temperature-range iron-based hardfacing flux-cored wire capable of resisting 650 DEG C and below
By using multi-component reinforced iron-based wear-resistant surfacing flux core welding wire, using the combination of high-carbon iron chromium, graphite and other components, the problem of insufficient hardness and wear resistance of traditional iron-based welding materials in high temperature environments is solved, and the problem of insufficient hardness and wear resistance of traditional iron-based welding materials in high temperature environments is realized. Good wear resistance below 650°C and reduce material costs.
Patent Information
- Application Number
- CN202411225435.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-12-06
AI Technical Summary
Traditional iron-based wear-resistant welding materials have reduced hardness and insufficient wear resistance in high temperature environments, which cannot meet the needs of 650℃ or above, and the high content of precious metals leads to an increase in material costs.
Iron-based wear-resistant overlayed flux core welding wire consisting of flux core powder wrapped with thin steel with outer skin. The flux core includes high-carbon ferrochrome, graphite, ferromolybdenum, ferroniobium, ferrovana, ferroniobium, ferrovana, ferrotitanium, ferrotungsten and ferrosilicon manganese The hardness and wear resistance are improved through multi-component reinforcement, with a filling rate of 35%-50%, and are prepared by mixing H08A thin steel strip with mechanical mixing.
Maintaining the average hardness of 45 to 53 HRC under a high temperature environment of 650℃ reduces the use of precious metals, effectively reduces the cost of materials, and fills the technical gap in iron-based wear-resistant surfacing coating in medium and low temperature environments.
Smart Images

Figure CN119077214A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of welding materials, and in particular to an iron-based wear-resistant surfacing flux-cored welding wire that can withstand a wide temperature range of 650°C or below. Background Art
[0002] With the development of industrial technology, the requirements for welding materials are increasing day by day. Especially under high temperature and high wear conditions, traditional wear-resistant cladding materials often cannot meet the requirements, and there are problems such as reduced hardness and reduced wear resistance, resulting in the use efficiency and service life of parts not being effectively improved. Therefore, it is of great practical significance to develop a flux-cored welding wire that can maintain excellent wear resistance in a wide temperature range.
[0003] At present, wear-resistant surfacing materials mainly include iron-based, nickel-based and cobalt-based alloys. Among them, although iron-based alloys have the advantages of low cost, good weldability, and good wettability with steel substrates, the heat resistance and wear resistance of their cladding layers need to be further improved. For example, the traditional high-chromium cast iron system wear-resistant surfacing coating can only serve in low-temperature environments not exceeding 350°C, and cannot meet the use requirements for medium temperatures (350-650°C) and above. Nickel-based alloys have excellent corrosion resistance and good high-temperature oxidation resistance, and are widely used in high-temperature environments of 650°C to 1000°C; similarly, cobalt-based alloys also have very excellent high-temperature wear resistance and are widely used as surface protective coatings for many key and major equipment parts. However, nickel and cobalt alloys are scarce metals and are expensive, which greatly increases material costs.
[0004] Patent document CN114523229A discloses an iron-based wear-resistant flux-cored welding wire and its preparation method and surfacing process. The flux-cored welding wire includes (by weight percentage): high carbon ferrochrome 0-10%, chromium powder 35-55%, manganese powder 1-7%, ferrosilicon 1-5%, nickel powder 10-16%, ferromolybdenum 1-7%, ferroniobium 1-7%, ferrovanadium 1-7%, chromium nitride 0-7%, and the balance is iron powder, with a filling rate of 35%-37%. The composition of the flux-cored welding wire belongs to the typical high chromium cast iron material, which is mainly composed of M3C, M7C3 and M 23 C6 and other hard carbides are used as dispersion strengthening phases. When used in high temperature wear-resistant applications, their average hardness is in the range of 42-47HRC, which is insufficient for the steel metallurgy and petrochemical smelting industries that require high high temperature wear resistance.
[0005] Patent document CN106238966A discloses a wear-resistant surfacing flux-cored welding wire, the flux core used includes the following raw materials by mass percentage: 5-10% titanium dioxide, 2-8% feldspar, 1-5% cryolite, 2-5% zircon, 2-8% rare earth silicon, 5-10% ferromanganese, 30-50% metallic chromium, 8-20% ferrotungsten, the balance is iron powder, and the filling rate is 20-40%. Although the average hardness of the surfacing layer of the iron-based wear-resistant flux-cored welding wire is within the range of 50-60HRC, which is suitable for 600℃ high temperature wear conditions, it adds a large amount of expensive pure chromium metal powder and ferrotungsten powder, resulting in a high cost of the welding wire, and it is not enough to meet the service requirements of about 650℃.
[0006] In addition, patent CN102240872A discloses a special welding rod for hot forging die surfacing repair and remanufacturing, the weight percentage of the chemical composition of its coating is: titanium dioxide 1-3%, marble 25-40%, fluorite 10-15%, quartz 3-5%, white clay 2-4%, high carbon ferrochrome 8-12%, high carbon ferromanganese 2-4%, ferrosilicon 2-4%, ferrotitanium 6-9%, ferromolybdenum 9-11%, cerium oxide 4-8%, metallic nickel 5-8%, graphite 1-2%; the welding core is H08A. The welding rod adopts Cr-Ni-Mo alloy system, the maximum content of high carbon ferrochrome in the welding rod coating is 12%, and the Cr content of the deposited metal is far less than 11%, which makes it difficult to ensure that the surfacing metal has sufficient wear resistance and oxidation resistance in a high temperature environment, and the use efficiency of the welding rod is far less than that of the welding wire with automatic continuous feeding. Summary of the invention
[0007] The purpose of the present invention is to provide an iron-based wear-resistant surfacing flux-cored welding wire with a wide temperature range of 650°C and below. The flux-cored welding wire of the present invention has low cost, and its surfacing layer can be applied to medium and low temperature (650°C and below) service environments, and has good wear resistance, so as to overcome the problems of insufficient high temperature hardness and wear resistance in the prior art.
[0008] To achieve the above object, the present invention adopts the following technical solutions:
[0009] The invention discloses an iron-based wear-resistant surfacing flux-cored welding wire with a wide temperature range of 650°C or below, which is composed of a thin steel strip outer skin and a flux core powder wrapped therein, wherein the flux core comprises the following raw materials in percentage by mass: 40% to 60% high-carbon ferrochromium, 1% to 6% graphite, 10% to 21% ferromolybdenum, 5% to 13% ferroniobium, 1% to 6% ferrovanadium, ≤2% ferrotitanium, 3% to 8% ferrotungsten, ≤3% ferrosilicon manganese, and the balance is iron powder.
[0010] Preferably, the core comprises the following raw materials in percentage by mass: 45% to 55% high carbon ferrochromium, 3% to 5% graphite, 14% to 19% ferromolybdenum, 7% to 11% ferroniobium, 2% to 5% ferrovanadium, ≤1.5% ferrotitanium, 4% to 7% ferrotungsten, 1% to 3% ferrosilicon manganese, and the remainder is iron powder.
[0011] The outer skin of the thin steel strip of the present invention is H08A, and the size of the steel strip is: 15-20 mm in width and 0.35-0.6 mm in thickness.
[0012] The high carbon ferrochrome contains 7wt% to 9wt% C and greater than or equal to 60wt% Cr, and the powder particle size is 60 to 325 meshes; C and Cr are transitioned to the cladding layer to form a hard carbide phase, which plays a major role in wear resistance.
[0013] The ferromolybdenum contains more than or equal to 60wt% of Mo; the powder particle size is 80-200 meshes; the Mo element is transitioned to the cladding layer to improve its hardenability, wear resistance and red hardness.
[0014] The ferroniobium contains greater than or equal to 50wt% of Nb, and the powder particle size is 60-200 meshes; the Nb element is transferred to the cladding layer to refine the grains and improve the high temperature hardness, wear resistance and oxidation resistance of the cladding layer.
[0015] The ferrovanadium contains 40wt% to 55wt% of V, and the particle size is 60 to 200 meshes; the V element is transferred to the surfacing layer to improve the heat resistance and wear resistance of the surfacing layer.
[0016] The titanium iron contains 35wt% to 45wt% Ti and less than 9wt% Al, and the powder particle size is 80 to 325 meshes; Ti and Al elements are transferred to the cladding layer, deoxidized, segregation is reduced, and the wear resistance of the cladding layer is improved.
[0017] The ferrotungsten contains 75wt% to 80wt% of W, and the particle size is 80 to 200 meshes; the W element is transferred to the cladding layer to improve the high temperature wear resistance of the cladding layer.
[0018] The ferrosilicomanganese contains 65wt% to 72wt% of Mn and 17wt% to 20wt% of Si, and the powder particle size is 60 to 325 meshes; the Si and Mn elements are transitioned to the cladding layer to achieve combined deoxidation and desulfurization, reduce the tendency of thermal cracking, and also play a role in solid solution strengthening and improving heat resistance.
[0019] The graphite contains 98wt% or more of C, and the powder particle size is 60-120 meshes; the C element is transferred to the cladding layer, and forms hard carbide with other metals, thereby improving the wear resistance of the cladding layer.
[0020] The iron powder is prepared by a reduction method, contains 99 wt% or more of Fe, and has a powder particle size of 60-200 meshes; the Fe element is transferred to the cladding layer to form the matrix structure of the cladding layer.
[0021] The iron-based wear-resistant cladding flux-cored welding wire of the present invention is made by wrapping H08A thin steel strip around mechanically mixed flux-cored powder on a flux-cored welding wire production line, and then undergoing multiple drawing and diameter reduction to finally produce a flux-cored welding wire with a diameter of 2.4 to 3.2 mm. The filling rate of the flux-cored welding wire (the percentage of flux-cored powder in the total weight of the flux-cored welding wire) is 35% to 50%.
[0022] After at least 2 layers of open arc cladding, the surface cladding metal contains the following alloy elements in percentage by mass: 4-6% C, 0.3-1.0% Si, 0.2-0.9% Mn, 18-24% Cr, 4-7% Mo, 0.3-0.8% Ti, 2-5% Nb, 0.8-1.6% V, 2.5-6.5% W, and the remainder is Fe.
[0023] The flux-cored welding wire cladding layer has a hardness of not less than 60HRC at room temperature, and an average hardness maintained within a range of 45 to 53HRC in a high temperature environment of 650°C.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] The invention provides an iron-based wear-resistant surfacing flux-cored welding wire with a wide temperature range of 650°C and below, which can reduce the use of precious metals and effectively reduce manufacturing costs. The room temperature hardness of not less than 60HRC can be achieved through multi-component strengthening, and the average hardness in a high temperature environment of 650°C is maintained in the range of 45 to 53HRC. In addition, the invention fills the technical gap of surface protection by iron-based wear-resistant surfacing coating in medium and low temperature environments between 350 and 650°C. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 The invention provides an iron-based wear-resistant surfacing flux-cored welding wire.
[0027] Figure 2 This is a SEM image of the microstructure of the cladding metal in Example 1 of the present invention. DETAILED DESCRIPTION
[0028] The present invention is described in detail below with reference to actual tooling conditions, but the present invention is not limited to these implementation cases. Unless otherwise specified, the raw materials involved in the present invention are purchased through commercial channels.
[0029] Embodiment 1:
[0030] The invention discloses an iron-based wear-resistant surfacing flux-cored welding wire, comprising a thin steel strip outer skin and a flux core powder, wherein the flux core is composed of the following raw materials in percentage by mass: 50% high-carbon ferrochromium, 3.8% graphite, 15.2% ferromolybdenum, 8.5% ferroniobium, 4.5% ferrovanadium, 1% ferrotitanium, 5% ferrotungsten, 2% ferrosilicon manganese and 10% iron powder.
[0031] Among them, high carbon ferrochromium contains 8.5wt% C, 65wt% Cr, and the powder particle size is 60-200 mesh. Ferromolybdenum contains 67wt% Mo, and the powder particle size is 80-120 mesh. Ferroniobium contains 53wt% Nb, and the powder particle size is 60-200 mesh. Ferrovanadium contains 50wt% V, and the particle size is 80-200 mesh. Ferrotitanium contains 40wt% Ti and 7.5wt% Al, and the powder particle size is 80-120 mesh. Ferrotungsten contains 75wt% W, and the particle size is 120-200 mesh. Ferrosilicomanganese contains 67wt% Mn and 20wt% Si, and the powder particle size is 60-200 mesh. Graphite contains 98wt% C, and the powder particle size is 60-120 mesh. Iron powder is prepared by reduction method, contains 99wt% Fe, and the powder particle size is 60-150 mesh.
[0032] On the flux-cored welding wire production line, H08A thin steel strip is wrapped with evenly mixed flux-cored powder, which is then drawn and reduced to produce flux-cored welding wire with a diameter of 2.8 mm and a filling rate of 48%.
[0033] After two layers of open arc surfacing, the main chemical composition of the outer surface of the surfacing layer is 4.8wt% C, 0.6wt% Si, 0.6wt% Mn, 19wt% Cr, 4.5wt% Mo, 0.4wt% Ti, 4.5wt% Nb, 1.5% V, 4.6% W, and the rest is Fe. The average hardness at room temperature is 60HRC, and the high temperature hardness at 650℃ is 47HRC. After 30min of high temperature friction and wear at 650℃, the wear loss is 31.6mg.
[0034] Embodiment 2:
[0035] The invention discloses an iron-based wear-resistant surfacing flux-cored welding wire, comprising a thin steel strip outer skin and a flux core powder, wherein the flux core is composed of the following raw materials in percentage by mass: 55% high-carbon ferrochromium, 4.3% graphite, 14.8% ferromolybdenum, 7.9% ferroniobium, 2.5% ferrovanadium, 1.4% ferrotitanium, 4.2% ferrotungsten, 1.5% ferrosilicon manganese and 8.4% iron powder.
[0036] Among them, high carbon ferrochromium contains 9wt% C, 68wt% Cr, and the powder particle size is 80-240 mesh. Ferromolybdenum contains 68wt% Mo, and the powder particle size is 80-150 mesh. Ferroniobium contains 60wt% Nb, and the powder particle size is 60-150 mesh. Ferrovanadium contains 52wt% V, and the particle size is 60-120 mesh. Ferrotitanium contains 42wt% Ti and 3.5wt% Al, and the powder particle size is 80-200 mesh. Ferrotungsten contains 77wt% W, and the particle size is 120-200 mesh. Ferrosilicomanganese contains 72wt% Mn and 17wt% Si, and the powder particle size is 80-240 mesh. Graphite contains 98.5wt% C, and the powder particle size is 80-120 mesh. Iron powder is prepared by reduction method, contains 99wt% Fe, and the powder particle size is 80-150 mesh.
[0037] On the flux-cored welding wire production line, H08A thin steel strip is wrapped with evenly mixed flux-cored powder, which is then drawn and reduced to produce flux-cored welding wire with a diameter of 2.8 mm and a filling rate of 49%.
[0038] After two layers of open arc surfacing, the main chemical composition of the outer surface of the surfacing layer is 5.1wt% C, 0.4wt% Si, 0.8wt% Mn, 22wt% Cr, 4.1wt% Mo, 0.6wt% Ti, 3.7wt% Nb, 1.2% V, 4.1% W, and the rest is Fe. The average hardness at room temperature is 64HRC, and the high temperature hardness at 650℃ is 52HRC. After 30min of high temperature friction and wear at 650℃, the wear loss is 26.3mg.
[0039] Embodiment 3:
[0040] The invention discloses an iron-based wear-resistant surfacing flux-cored welding wire, comprising a thin steel strip outer skin and a flux core powder, wherein the flux core is composed of the following raw materials in percentage by mass: 58% high-carbon ferrochromium, 5.2% graphite, 17.3% ferromolybdenum, 5.5% ferroniobium, 1.5% ferrovanadium, 0.8% ferrotitanium, 3.5% ferrotungsten, 0.7% ferrosilicon manganese and 7.5% iron powder.
[0041] Among them, high carbon ferrochromium contains 9wt% C, 69wt% Cr, and the powder particle size is 80-325 mesh. Ferromolybdenum contains 70wt% Mo, and the powder particle size is 80-150 mesh. Ferroniobium contains 65wt% Nb, and the powder particle size is 80-200 mesh. Ferrovanadium contains 55wt% V, and the particle size is 80-200 mesh. Ferrotitanium contains 45wt% Ti and 5.5wt% Al, and the powder particle size is 80-240 mesh. Ferrotungsten contains 79wt% W, and the particle size is 80-150 mesh. Ferrosilicomanganese contains 72wt% Mn and 19wt% Si, and the powder particle size is 60-240 mesh. Graphite contains 98.5wt% C, and the powder particle size is 60-120 mesh. Iron powder is prepared by reduction method, contains 99.5wt% Fe, and the powder particle size is 80-200 mesh.
[0042] On the flux-cored welding wire production line, H08A thin steel strip is wrapped with evenly mixed flux-cored powder, which is then drawn and reduced to produce flux-cored welding wire with a diameter of 2.4 mm and a filling rate of 38%.
[0043] After two layers of open arc surfacing, the main chemical composition of the outer surface of the surfacing layer is 5.4wt%C, 0.5wt%Si, 0.9wt%Mn, 23wt%Cr, 6.1wt%Mo, 0.7wt%Ti, 3.0wt%Nb, 0.8%V, 3.3%W, and the rest is Fe. The average hardness at room temperature is 61HRC, and the high temperature hardness at 650℃ is 49HRC. After 30min of high temperature friction and wear at 650℃, the wear loss is 29.1mg.
[0044] The above is only a preferred embodiment of the present invention. It should be pointed out that the present invention is not limited to the above embodiments. Without departing from the technical principles of the present invention, various changes can be made according to the invention purpose of the present invention. Any changes, modifications, substitutions, combinations, and simplifications made according to the spirit and principles of the technical solution of the present invention should be regarded as equivalent replacement methods, and these changes also belong to the protection scope of the present invention.
Claims
1. A wide temperature range iron-based wear-resistant cladding flux-cored welding wire resistant to 650°C and below, characterized in that: The invention comprises a thin steel strip outer skin and a flux core powder, wherein the flux core comprises the following raw materials in percentage by mass: 40% to 60% high carbon ferrochromium, 1% to 6% graphite, 10% to 21% ferromolybdenum, 5% to 13% ferroniobium, 1% to 6% ferrovanadium, ≤2% ferrotitanium, 3% to 8% ferrotungsten, ≤3% ferrosilicon manganese, and the remainder is iron powder.
2. The iron-based wear-resistant cladding flux-cored welding wire with a wide temperature range of 650°C and below according to claim 1, characterized in that: The core comprises the following raw materials in percentage by mass: 45% to 55% high carbon ferrochromium, 3% to 5% graphite, 14% to 19% ferromolybdenum, 7% to 11% ferroniobium, 2% to 5% ferrovanadium, ≤1.5% ferrotitanium, 4% to 7% ferrotungsten, 1% to 3% ferrosilicon manganese, and the remainder is iron powder.
3. The iron-based wear-resistant cladding flux-cored welding wire with a wide temperature range of 650°C or below according to claim 1 or 2, characterized in that: The high carbon ferrochrome contains 7wt% to 9wt% C and 60wt% or more Cr, and the powder particle size is 60 to 325 meshes; the ferromolybdenum contains 60wt% or more Mo, and the powder particle size is 80 to 200 meshes.
4. The iron-based wear-resistant cladding flux-cored welding wire with a wide temperature range of 650°C or below according to claim 1 or 2, characterized in that: The ferroniobium contains greater than or equal to 50wt% of Nb, and the powder particle size is 60-200 meshes; the ferrovanadium contains 40wt%-55wt% of V, and the particle size is 60-200 meshes.
5. The iron-based wear-resistant cladding flux-cored welding wire with a wide temperature range of 650°C or below according to claim 1 or 2, characterized in that: The titanium iron contains 35wt% to 45wt% of Ti and less than 9wt% of Al, and the powder particle size is 80 to 325 meshes; the tungsten iron contains 75wt% to 80wt% of W, and the particle size is 80 to 200 meshes.
6. The iron-based wear-resistant cladding flux-cored welding wire with a wide temperature range of 650°C or below according to claim 1 or 2, characterized in that: The ferrosilicomanganese contains 65wt% to 72wt% of Mn and 17wt% to 20wt% of Si, and the powder particle size is 60 to 325 meshes; the graphite contains greater than or equal to 98wt% of C, and the powder particle size is 60 to 120 meshes; the iron powder is prepared by a reduction method, contains greater than or equal to 99wt% of Fe, and the powder particle size is 60 to 200 meshes.
7. The iron-based wear-resistant cladding flux-cored welding wire with a wide temperature range of 650°C or below according to claim 1 or 2, characterized in that: The thin steel strip is H08A thin steel strip.
8. The iron-based wear-resistant cladding flux-cored welding wire with a wide temperature range of 650°C or below according to claim 1 or 2, characterized in that: The diameter of the flux-cored welding wire is 2.4-3.2 mm; the filling rate of the flux-cored welding wire is 35%-50%.
9. The iron-based wear-resistant cladding flux-cored welding wire with a wide temperature range of 650°C or below according to claim 1 or 2, characterized in that: After at least 2 layers of open arc cladding, the surface cladding metal contains the following alloy elements in percentage by mass: 4% to 6% C, 0.3% to 1.0% Si, 0.2% to 0.9% Mn, 18% to 24% Cr, 4% to 7% Mo, 0.3% to 0.8% Ti, 2% to 5% Nb, 0.8% to 1.6% V, 2.5% to 6.5% W, and the balance is Fe.
10. The iron-based wear-resistant cladding flux-cored welding wire with a wide temperature range of 650°C or below according to claim 1 or 2, characterized in that: The service environment of the flux-cored welding wire cladding layer is not less than 60HRC under room temperature conditions, and the average hardness is maintained in the range of 45 to 53HRC under a high temperature environment of 650°C.
Citation Information
Cited By
Iron-based alloy composite wear-resistant material for preparing roller sleeve flux-cored wire
CN119549931A
Hardfacing flux-cored wire for repairing surface of single-tooth roller
CN120816192A
A wear-resistant flux-cored welding wire for surface repair of flux-cored and single-toothed rollers, and a welding method.
CN120816192B