X90 pipeline steel with good low-temperature toughness in heat affected zone of welded joint and preparation method of X90 pipeline steel

By optimizing the alloy composition and preparation process of X90 pipeline steel, especially the synergistic effect of microalloying elements, the problem of insufficient low-temperature toughness in the heat-affected zone of welded joints has been solved, realizing high-strength and high-toughness welded joints suitable for long-distance pipeline construction, with the advantages of low cost and high-efficiency production.

CN118880175APending Publication Date: 2024-11-01PIPECHINA SOUTH CHINA CO +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410958275.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

In the existing technology, the heat-affected zone of welded joints of X90 pipeline steel has the problem of insufficient low-temperature toughness, unreasonable alloy composition, low strength and toughness, and poor welding performance.

Method used

By optimizing the base alloy composition of X90 pipeline steel and utilizing the synergistic effect of microalloying elements such as Nb, V, Ti, Ni, and Mo, combined with solid solution strengthening, precipitation strengthening, grain refinement strengthening, and dislocation strengthening, X90 pipeline steel with optimized chemical composition was prepared. The microstructure and mechanical properties were then controlled through steps such as smelting, continuous casting, slab heating, rough rolling, finish rolling, controlled cooling, coiling, and tempering.

Benefits of technology

It significantly improves the low-temperature toughness of the heat-affected zone of welded joints, enhances the strength and toughness of X90 pipeline steel, is suitable for long-distance pipeline construction, provides material support for energy strategic security, and has low production cost and high efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118880175A_ABST
    Figure CN118880175A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of high-grade pipeline steel manufacturing, in particular to X90 pipeline steel with good low-temperature toughness in a heat affected zone of a welded joint and a preparation method. The alloy comprises the following chemical components in percentage by mass: 0.040 to 0.060 percent of C, 0.10 to 0.20 percent of Si, 1.75 to 1.95 percent of Mn, less than or equal to 0.015 percent of P, less than or equal to 0.0040 percent of S, 0.20 to 0.30 percent of Ni, 0.25 to 0.30 percent of Cr, 0.05 to 0.15 percent of Mo, 0.030 to 0.060 percent of Nb, 0.030 to 0.060 percent of V, 0.010 to 0.030 percent of Ti, 0.25 to 0.30 percent of Cu, 0.03 to 0.06 percent of Al, less than or equal to 0.21 percent of Pcm and 0.38 to 0.47 percent of Ceq. According to the method, the microscopic structure and the mechanical property are regulated and controlled, the obdurability is improved, the production cost is low, and the production efficiency is high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of high-level pipeline steel manufacturing, and in particular to X90 pipeline steel with good low-temperature toughness in a heat-affected zone of a welded joint and a preparation method thereof. Background Art

[0002] As one of the main energy transportation industries, oil and gas pipelines play a very important role in the national economy. With the growth of oil and gas demand worldwide, the second-generation pipeline steel (X70 / X80) has been unable to meet the transportation requirements in recent years. In order to meet the design requirements of a transportation pressure greater than 12MPa, the third-generation pipeline steel (X90 / X100) will become the main steel for pipeline transportation in the future. X90 pipeline steel is a controlled-rolled and controlled-cooled low-carbon microalloy steel with high strength and good resistance to ductile fracture.

[0003] The welding process of pipeline steel is a non-equilibrium process of rapid heating and rapid cooling. During the welding process of pipe making and steel pipe connection, the structure and performance of the weld heat affected zone will change significantly due to the effect of thermal cycle, which will significantly affect the operation safety of the pipeline. Therefore, the weld heat affected zone has always been the focus of pipeline steel research. With the increase of strength, the weld heat affected zone is more likely to have problems such as softening and embrittlement.

[0004] At present, there are some studies on the rolling process and welding process of X90 pipeline steel at home and abroad. After searching, some patents and documents were found, but the relevant contents all focused on the manufacturing technology of X90 submerged arc welded pipe, the production and manufacturing of girth weld gas shielded solid welding wire and welding process, etc. At the same time, the metallurgical composition, manufacturing method and mechanical properties of the welding heat affected zone of the product described in the present invention are obviously different from those of other patents or documents. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide X90 pipeline steel with good low-temperature toughness in the heat-affected zone of the welded joint and a preparation method thereof, so as to solve the problems of unreasonable alloy composition, low strength and toughness, and poor welding performance of the steel in the prior art.

[0006] The technical solution of the present invention to solve the above technical problems is as follows:

[0007] The invention provides an X90 pipeline steel with good low-temperature toughness in a heat-affected zone of a welded joint. The chemical composition of the X90 pipeline steel comprises, by mass percentage, C 0.040-0.060%, Si 0.10-0.20%, Mn 1.75-1.95%, P≤0.015%, S≤0.0040%, Ni 0.20-0.30%, Cr 0.25-0.30%, Mo0.05-0.15%, Nb 0.030-0.060%, V0.030-0.060%, Ti 0.010-0.030%, Cu0.25-0.30%, Al 0.03-0.06%, weld crack sensitivity coefficient Pcm≤0.21%, carbon equivalent Ceq0.38-0.47%, and the remainder is Fe and unavoidable impurities.

[0008] Based on the above technical solution, the present invention can also be improved as follows.

[0009] Further, the carbon equivalent Ceq is calculated as follows:

[0010] Ceq=[C]+[Mn] / 6+([Cr]+[Mo]) / 5+([Ni]+[Cu]) / 15, where [C], [Mn], [Cr], [Mo], [Ni], and [Cu] represent the mass percentages of the corresponding elements respectively;

[0011] The calculation method of the weld crack sensitivity coefficient Pcm is:

[0012] Pcm=[C]+[Si] / 30+([Mn]+[Cu]+[Cr]) / 20+[Ni] / 60+[Mo] / 15+[V] / 10+5[B], wherein [C], [Si], [Mn], [Cu], [Cr], [Ni], [Mo], [V], and [B] respectively represent the mass percentages of the corresponding elements. When the mass percentage content of B in the impurities is less than 0.001%, the value of [B] is 0.

[0013] Furthermore, at room temperature, the yield strength of the X90 pipeline steel is 663MPa-688MPa, the tensile strength is 780MPa-815MPa, the yield strength ratio is 0.84-0.86, the Charpy impact energy at -20°C is 306J-320J, and the DWTT performance at -15°C is 94%-100%.

[0014] Furthermore, the average value of the -10°C Charpy impact energy of the heat affected zone of the girth weld joint of the X90 pipeline steel is 266 J to 278 J, and the value of the CTOD at -10°C is 0.86 to 0.92 mm.

[0015] The present invention also provides a method for preparing X90 pipeline steel with good low-temperature toughness in the heat-affected zone of the welded joint as mentioned above, wherein the X90 pipeline steel is prepared through the steps of smelting, continuous casting, slab heating, rough rolling, finish rolling, controlled cooling, coiling, and tempering.

[0016] Further, the method further comprises the following steps:

[0017] S1. Smelting to obtain pure molten steel;

[0018] S2, continuously casting the pure molten steel to obtain a slab;

[0019] S3, heating the slab, the furnace temperature is 1150-1250° C., and the heating time is 180-280 min;

[0020] S4, performing multiple passes of rough rolling on the heated slab to obtain an intermediate slab, wherein the reduction ratio of the last pass is greater than or equal to 25%, and the temperature of the last pass is 900-950° C.;

[0021] S5, performing multiple passes of finish rolling on the intermediate billet to obtain a hot-rolled steel strip of target thickness; wherein the inlet temperature of the finish rolling is less than or equal to 920° C., and the cumulative reduction of the finish rolling is greater than or equal to 65% of the thickness of the intermediate billet;

[0022] S6, rapidly cooling the hot-rolled steel strip to 400-420°C, the cooling time being 10-15s, and the cooling rate being 15-20°C / s;

[0023] S7, coiling the cooled hot-rolled steel strip to obtain a steel coil, wherein the coiling temperature is 350° C. to 400° C.;

[0024] S8. Performing tempering heat treatment on the steel coil, wherein the tempering heat treatment is to heat the steel coil to 450-500° C., keep the temperature for 2-3 hours, and then cool the steel coil to obtain the steel material.

[0025] Furthermore, in step S1, the smelting sequentially includes the steps of converter smelting, LF and RH refining.

[0026] Furthermore, in step S2, the continuous casting process adopts a low superheat of 15 to 25°C above the liquidus, a low pulling speed of 1.0 to 1.5 m / min and a dynamic light reduction process with a total reduction of 6 to 8 mm, and the thickness of the slab is 220 to 260 mm.

[0027] Further, in step S4, the rolling passes are 5, and in step S5, the rolling passes are 7.

[0028] Further, in step S4, the thickness of the intermediate blank is greater than or equal to 50 mm.

[0029] The beneficial effects of the present invention are:

[0030] (1) The X90 pipeline steel of the present invention has good low-temperature toughness in the heat-affected zone of the welded joint, and can further improve the mechanical properties, especially the low-temperature toughness, of the corresponding weld heat-affected zone by optimizing the alloy composition, microstructure and mechanical properties of the base material of the X90 pipeline steel;

[0031] (2) The X90 pipeline steel with good low-temperature toughness in the heat-affected zone of the welded joint of the present invention can be more suitable for long-distance pipeline construction and provide material support for energy strategic security;

[0032] (3) The method for preparing X90 pipeline steel with good low-temperature toughness in the heat-affected zone of the welded joint of the present invention optimizes the alloy composition, regulates the microstructure and mechanical properties of the X90 pipeline steel through innovative design of rolling and heat treatment processes, and improves the strength and toughness of the X90 pipeline steel from two aspects: grain refinement and second phase regulation;

[0033] (4) The method for preparing X90 pipeline steel with good low-temperature toughness in the heat-affected zone of the welded joint of the present invention also has the advantages of low production cost and high production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 The metallographic structure diagram of Example 2 is X90 pipeline steel with good low-temperature toughness in the heat-affected zone of the welded joint of the present invention. Figure 1 A in the middle is the cross-sectional metallographic structure diagram. Figure 1 Middle B is a longitudinal section for organization chart;

[0035] Figure 2 The X90 pipeline steel of the present invention has good low-temperature toughness in the heat-affected zone of the welded joint. The TEM image of the (Nb, Mo)C dispersion precipitation in Example 2 during the cooling stage after fine rolling is as follows: Figure 2 A in the middle is a TEM image of nanoscale dispersed precipitation. Figure 2 B is the TEM image of (Nb, Mo)C. Figure 2 C is Figure 2 EDS spectrum of selected area 1 in B;

[0036] Figure 3 The X90 pipeline steel of the present invention has good low-temperature toughness in the heat-affected zone of the welded joint. The microstructure metallographic diagram of the heat-affected zone of Example 2 after welding is shown in FIG. Figure 3 A in the middle is the coarse grain area. Figure 3 B in the middle is the fine boundary area. Figure 3 C is the critical section. Figure 3 D in the middle is the tempering zone;

[0037] Figure 4 The X90 pipeline steel of the present invention has good low-temperature toughness in the heat-affected zone of the welded joint. The SEM images of different positions of the weld heat-affected zone after welding in Example 2 are as follows: Figure 4 A in the middle is the coarse grain area. Figure 4 B in the middle is the fine boundary area. Figure 4 C is the critical section. Figure 4 D in the middle is the tempering zone. DETAILED DESCRIPTION

[0038] The principles and features of the present invention are described below in conjunction with the accompanying drawings. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention.

[0039] The X90 pipeline steel with good low-temperature toughness in the heat-affected zone of the welded joint of the present invention comprises, by mass percentage, the following chemical components: C 0.040-0.060%, Si 0.10-0.20%, Mn 1.75-1.95%, P≤0.015%, S≤0.0040%, Ni 0.20-0.30%, Cr 0.25-0.30%, Mo 0.05-0.15%, Nb 0.030-0.060%, V 0.030-0.060%, Ti 0.010-0.030%, Cu 0.25-0.30%, Al 0.03-0.06%, weld crack sensitivity coefficient Pcm≤0.21%, carbon equivalent Ceq 0.38-0.47%, and the remainder being Fe and unavoidable impurities.

[0040] The X90 pipeline steel with good low-temperature toughness in the heat-affected zone of the welded joint of the present invention can effectively improve the strength and toughness of the X90 pipeline steel through reasonable alloy element design, especially through the synergistic effect of micro-alloy elements such as Nb, V, Ti, Ni and Mo, combined with solid solution strengthening, precipitation strengthening, fine grain strengthening and dislocation strengthening.

[0041] The carbon equivalent Ceq is calculated as follows:

[0042] Ceq=[C]+[Mn] / 6+([Cr]+[Mo]) / 5+([Ni]+[Cu]) / 15,

[0043] Wherein [C], [Mn], [Cr], [Mo], [Ni], and [Cu] represent the mass percentages of the corresponding elements respectively;

[0044] The calculation method of weld crack sensitivity coefficient Pcm is as follows:

[0045] Pcm=[C]+[Si] / 30+([Mn]+[Cu]+[Cr]) / 20+[Ni] / 60+[Mo] / 15+[V] / 10+5[B], wherein [C], [Si], [Mn], [Cu], [Cr], [Ni], [Mo], [V], and [B] respectively represent the mass percentages of the corresponding elements. When the mass percentage content of B in the impurities is less than 0.001%, the value of [B] is 0.

[0046] Preferably, at room temperature, the yield strength of X90 pipeline steel is 663MPa-688MPa, the tensile strength is 780MPa-815MPa, the yield strength ratio is 0.84-0.86, the Charpy impact energy at -20°C is 306J-320J, and the DWTT performance at -15°C is 94%-100%.

[0047] Preferably, the X90 pipeline steel or the steel pipe prepared using the X90 pipeline steel has an average value of -10°C Charpy impact energy of the heat affected zone of the girth weld joint of 266 J to 278 J, and a CTOD value of 0.86 to 0.92 mm at -10°C.

[0048] The method for preparing X90 pipeline steel with good low-temperature toughness in the heat-affected zone of a welded joint of the present invention is prepared through the steps of smelting, continuous casting, slab heating, rough rolling, finish rolling, controlled cooling, coiling and tempering.

[0049] The method specifically comprises the following steps:

[0050] S1. Smelting to obtain pure molten steel.

[0051] Preferably, the specific smelting process includes converter smelting, LF and RH refining to obtain pure molten steel with target metallurgical composition and low P and low S impurity elements.

[0052] S2, continuously casting the pure molten steel to obtain a slab;

[0053] Preferably, the continuous casting process is: pure molten steel is cast in a protective manner, and during the continuous casting process, a low superheat of 15 to 25°C above the liquidus, a low pulling speed of 1.0 to 1.5 m / min, and a dynamic light reduction process with a total reduction of 6 to 8 mm are adopted to finally obtain a slab with a thickness of 220 to 260 mm.

[0054] Preferably, the thickness of the slab finally obtained is 240 mm.

[0055] S3. The slab is heated to a furnace temperature of 1150 to 1250° C. for a heating time of 180 to 280 minutes.

[0056] S4, the heated slab is subjected to multiple rough rolling to obtain an intermediate slab, wherein the reduction ratio of the last pass is greater than or equal to 25%, and the reduction ratio refers to (slab thickness of the previous pass - slab thickness of the current pass) / slab thickness of the previous pass * 100%. The temperature of the last rolling is 900-950°C.

[0057] Preferably, in step S4, the thickness of the intermediate blank is greater than or equal to 50 mm.

[0058] S5. Perform multiple passes of finish rolling on the intermediate billet to obtain a hot-rolled steel strip of target thickness; wherein the inlet temperature of the finish rolling is less than or equal to 920° C., and the cumulative reduction of the finish rolling is greater than or equal to 65% of the thickness of the intermediate billet.

[0059] Preferably, in step S4, the rolling passes are 5, and in step S5, the rolling passes are 7.

[0060] The setting of the rough rolling and finish rolling passes and the reduction rate effectively reduces the production cost of the method of the present invention, and adopts the TMCP process flow to improve the production efficiency of batch industrial production of X90 pipeline steel.

[0061] S6. Rapidly cool the hot-rolled steel strip to 400-420°C, with a cooling time of 10-15s and a cooling rate of 15-20°C / s.

[0062] S7, coiling the cooled hot-rolled steel strip to obtain a steel coil, wherein the coiling temperature is 350° C. to 400° C.;

[0063] S8. Performing tempering heat treatment on the steel coil. The tempering heat treatment includes heating the steel coil to 450-500° C., keeping the temperature for 2-3 hours, and cooling the steel coil to obtain the X90 pipeline steel.

[0064] Preferably, after keeping the temperature for 2 to 3 hours, the steel coil is cooled to room temperature to complete the cooling.

[0065] The above-mentioned preparation process of the present invention controls the temperature precisely through continuous casting, rough rolling, finishing rolling, controlling the temperature and speed of rapid cooling, coiling and tempering process, and realizes the dispersion precipitation of micro-alloy carbides such as (Nb, Mo) C, so that the content of acicular ferrite, granular bainite and polygonal ferrite in X90 pipeline steel can be effectively regulated. The above-mentioned preparation method can refine the grains, increase the density of large-angle grain boundaries, and improve the crack resistance of X90 pipeline steel. Because the organization is hereditary, after the fully automatic ring welding process, the acicular ferrite content in the heat-affected zone increases, and the low-temperature toughness of the welding heat-affected zone is improved.

[0066] The effects of the present invention are illustrated below by means of specific embodiments.

[0067] Three groups of X90 pipeline steels with different alloying elements are selected within the set alloying element range as Examples 1 to 3, and are respectively recorded as 1#, 2# and 3#. At the same time, comparative examples 4 and 5 are set, recorded as 4# and 5#, and the alloying elements of the comparative examples are outside the set range. By setting different slab heating temperatures, heating and holding times, rough rolling and finishing rolling temperatures, and measuring the mechanical properties of the embodiments and comparative examples under different rolling process conditions. The metallurgical compositions of each embodiment and comparative example are shown in Tables 1 and 2, and the specific preparation process parameters are shown in Tables 3 and 4.

[0068] Table 1 Metallurgical composition of X90 pipeline steel of Examples 1 to 3 (wt.%)

[0069]

[0070] Wherein, Ceq=C+Mn / 6+(Cr+Mo) / 5+(Ni+Cu) / 15;

[0071] Pcm=C+Si / 30+(Mn+Cu+Cr) / 20+Ni / 60+Mo / 15+V / 10+5B.

[0072] Table 2 Metallurgical composition of comparative examples 4 and 5 (wt.%)

[0073]

[0074] Table 3 X90 pipeline steel manufacturing process parameters of Examples 1 to 3

[0075]

[0076] Table 4 Steel manufacturing process parameters of Comparative Examples 4 and 5

[0077]

[0078] The mechanical properties and girth weld performance tests were performed on the steels of Examples 1 to 3 and Comparative Examples 4 to 5, respectively. The test results are shown in Tables 5 to 8.

[0079] Table 5 Mechanical properties of X90 pipeline steel pipes of Examples 1 to 3

[0080]

[0081] Table 6 Mechanical properties of steel materials in Comparative Examples 4 and 5

[0082]

[0083] The mechanical properties of the ring welds of the embodiments of the present invention and the comparative examples are shown in Tables 7 and 8.

[0084] Table 7 Mechanical properties of X90 pipeline steel girth welds of Examples 1 to 3

[0085]

[0086] Table 8 Mechanical properties of steel belt ring welds of comparative examples 4 and 5

[0087]

[0088] The metallographic structure of the X90 pipeline steel in Example 2 is as follows: Figure 1 As shown in the figure, after finishing rolling, the TEM image of (Nb, Mo)C dispersion precipitation in the cooling stage is as follows Figure 2 After welding, the X90 pipeline steel of Example 1 has a microstructure in the heat affected zone as shown in FIG. Figure 3 As shown in the figure, the SEM images of different positions affected by welding heat after welding are as follows Figure 4 shown.

[0089] By comparing the metallurgical compositions of the embodiments and comparative examples in Tables 1 and 2 and combining the measured mechanical properties, it is found that the strength and impact toughness of the embodiments are significantly higher than those of the comparative examples. Figures 1 to 4 As shown, the microalloying element design of the 2# pipeline steel in Example 2 is the most reasonable. After 5 rough rolling and 7 finish rolling, the cooling rate is 15-20°C / s. The reasonable controlled rolling and controlled cooling process is combined with the tempering and heat preservation treatment to produce dispersed precipitation of (Nb, Mo)C in the X90 pipeline steel, which precipitates and pins the grain boundaries. Combined with the solid solution drag effect of Ti and Ni elements, the purpose of grain refinement is achieved, the strength and impact toughness are improved, and finally a good strength-toughness match is achieved.

[0090] For the heating temperature and holding time, the heating temperature of the slab should not be set too high, otherwise it will cause the original austenite grains to grow rapidly, the grain boundaries to be coarse, and the MA components in the structure to be obviously coarsened, causing local stress concentration. After the controlled rolling and controlled cooling process, microcracks are easily induced at the coarsened MA components, resulting in the strength and toughness of the comparative example to be lower than that of the embodiment.

[0091] After fully automatic girth welding, the impact toughness of the weld area in each embodiment is slightly lower than the impact toughness value of the parent material, but significantly higher than the comparative examples. Since the parent material structure is hereditary, the X90 pipeline steel embodiment has a good match of strength and toughness. Therefore, after the welding heat cycle, the organizational properties of the welding heat affected zone are excellent. Therefore, the impact toughness of the welding heat affected zone of the embodiment is better than that of the comparative example. This shows that the innovative design of the metallurgical composition and heat treatment rolling process of the present invention can effectively improve the mechanical properties of the X90 pipeline steel and its heat affected zone after the girth welding process, and the corresponding microstructure is significantly optimized, and the product has good performance.

[0092] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. An X90 pipeline steel with good low-temperature toughness in the heat-affected zone of a welded joint, characterized in that: Its chemical composition, in mass percentage, includes: C 0.040-0.060%, Si 0.10-0.20%, Mn 1.75-1.95%, P≤0.015%, S≤0.0040%, Ni 0.20-0.30%, Cr 0.25-0.30%, Mo0.05-0.15%, Nb 0.030-0.060%, V0.030-0.060%, Ti 0.010-0.030%, Cu0.25-0.30%, Al 0.03-0.06%, weld crack sensitivity coefficient Pcm≤0.21%, carbon equivalent Ceq0.38-0.47%, and the rest is Fe and unavoidable impurities.

2. The X90 pipeline steel with good low temperature toughness in the heat affected zone of the welded joint according to claim 1, characterized in that: The carbon equivalent Ceq is calculated as follows: Ceq = [C] + [Mn] / 6 + ([Cr] + [Mo]) / 5 + ([Ni] + [Cu]) / 15, wherein [C], [Mn], [Cr], [Mo], [Ni], and [Cu] represent the mass percentages of the corresponding elements, respectively; The calculation method of the weld crack sensitivity coefficient Pcm is: Pcm=[C]+[Si] / 30+([Mn]+[Cu]+[Cr]) / 20+[Ni] / 60+[Mo] / 15+[V] / 10+5[B], wherein [C], [Si], [Mn], [Cu], [Cr], [Ni], [Mo], [V], and [B] respectively represent the mass percentages of the corresponding elements. When the mass percentage content of B in the impurities is less than 0.001%, the value of [B] is 0.

3. The X90 pipeline steel with good low temperature toughness in the heat affected zone of the welded joint according to claim 1 or 2, characterized in that: At room temperature, the yield strength of the X90 pipeline steel is 663MPa-688MPa, the tensile strength is 780MPa-815MPa, the yield strength ratio is 0.84-0.86, the Charpy impact energy at -20°C is 306J-320J, and the DWTT performance at -15°C is 94%-100%.

4. The X90 pipeline steel with good low temperature toughness in the heat affected zone of the welded joint according to claim 1 or 2, characterized in that: The average value of the -10°C Charpy impact energy of the heat affected zone of the girth weld of the X90 pipeline steel is 266 J to 278 J, and the value of the CTOD at -10°C is 0.86 to 0.92 mm.

5. A method for preparing X90 pipeline steel with good low-temperature toughness in the heat-affected zone of a welded joint as claimed in any one of claims 1 to 4, characterized in that: The X90 pipeline steel is prepared through the steps of smelting, continuous casting, slab heating, rough rolling, finish rolling, controlled cooling, coiling and tempering.

6. The method for preparing X90 pipeline steel with good low-temperature toughness in the heat-affected zone of the welded joint according to claim 5, characterized in that: The following steps are also included: S1. Smelting to obtain pure molten steel; S2, continuously casting the pure molten steel to obtain a slab; S3, heating the slab, the furnace temperature is 1150-1250° C., and the heating time is 180-280 min; S4, performing multiple passes of rough rolling on the heated slab to obtain an intermediate slab, wherein the reduction ratio of the last pass is greater than or equal to 25%, and the temperature of the last pass is 900-950° C.; S5, performing multiple passes of finish rolling on the intermediate billet to obtain a hot-rolled steel strip of target thickness; wherein the inlet temperature of the finish rolling is less than or equal to 920° C., and the cumulative reduction of the finish rolling is greater than or equal to 65% of the thickness of the intermediate billet; S6, rapidly cooling the hot-rolled steel strip to 400-420° C., the cooling time is 10-15 seconds, and the cooling rate is 15-20° C. / s; S7, coiling the cooled hot-rolled steel strip to obtain a steel coil, wherein the coiling temperature is 350° C. to 400° C.; S8. Performing tempering heat treatment on the steel coil, wherein the tempering heat treatment is to heat the steel coil to 450-500° C., keep the temperature for 2-3 hours, and then cool the steel coil to obtain the X90 pipeline steel.

7. The method for preparing X90 pipeline steel with good low-temperature toughness in the heat-affected zone of a welded joint according to claim 6, characterized in that: In step S1, the smelting includes the steps of converter smelting, LF and RH refining in sequence.

8. The method for preparing X90 pipeline steel with good low-temperature toughness in the heat-affected zone of a welded joint according to claim 6, characterized in that: In step S2, the continuous casting process adopts a low superheat of 15 to 25°C above the liquidus, a low pulling speed of 1.0 to 1.5 m / min, and a dynamic soft reduction process with a total reduction of 6 to 8 mm, and the thickness of the slab is 220 to 260 mm.

9. The method for preparing X90 pipeline steel with good low-temperature toughness in the heat-affected zone of a welded joint according to claim 6, characterized in that: In step S4, the rolling passes are 5 times, and in step S5, the rolling passes are 7 times.

10. The method for preparing X90 pipeline steel with good low-temperature toughness in the heat-affected zone of a welded joint according to claim 9, characterized in that: In step S4, the thickness of the intermediate blank is greater than or equal to 50 mm.